Cold pressing die for aluminum alloy rib web structure forgings and capped cold pressing method

Through the capped cold pressing method, the design of the cold pressing die is used to press only the ribs of the aluminum alloy forgings, which solves the problems of the traditional cold pressing method that the ribs are not pressed through and the tensile stress in the interface area of ​​the web is large, and the 7xxx system is realized. The residual stress of aluminum alloy forgings is eliminated, significantly improving the mechanical properties and fatigue life.

CN118744192APending Publication Date: 2024-10-08CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD

Patent Information

Application Number
CN202411040475.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

7xxx series aluminum alloy forgings produce large residual stress after solution quenching, resulting in processing deformation and reduced fatigue life. The traditional cold pressing method has the problems of impermeable ribs and high tensile stress in the interface area between the web and ribs.

Method used

The capped cold pressing method of aluminum alloy rib web structure-type forgings is used. By designing a cold-pressed fillet between the cold-pressed side wall and the cold-pressed top wall of the cold-pressing mold, the rib side wall has a draft angle and ribs. The corners of the strips are rounded, and only the ribs are pressed during the cold pressing process to maintain the gap between the web and the ribs, avoid cold pressing of the web, and control the amount of cold pressing within 1%-5% of the height of the ribs. The speed is 0.2~1mm/s.

Benefits of technology

It effectively avoids the problem of the tightness of the ribs, reduces the tensile stress in the interface area between the web and the ribs, achieves a better residual stress elimination effect, and significantly reduces the residual stress by nearly 50%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744192A_ABST
    Figure CN118744192A_ABST
Patent Text Reader

Abstract

The invention discloses a cold pressing die for an aluminum alloy rib web structure forge piece and a cap type cold pressing method, belongs to the field of residual stress control of die forge pieces, and aims to effectively reduce residual stress. The cold pressing die comprises a rib cold pressing part corresponding to the rib and a web cold pressing part corresponding to the web; the rib cold pressing part is a cavity defined by cold pressing side walls on the two sides and a cold pressing top wall. When the rib top of the rib is cold-pressed by the cold-pressing top wall, a gap D is formed between the web cold-pressing part and the web of the forge piece, D is equal to 5-15mm, a negative gap is formed between the cold-pressing fillet of the rib cold-pressing part and the rib fillet, and the cold-pressing fillet of the rib cold-pressing part is cold-pressed with the rib fillet. During cold pressing, only the ribs are pressed, and the web is not pressed. According to the capped cold pressing method for the forge piece with the aluminum alloy rib web structure, the ribs of the aluminum alloy forge piece are pressed thoroughly by only pressing the ribs and not pressing the web, the cold pressing amount is relatively uniform, and meanwhile the good residual stress eliminating effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of residual stress control of die forgings, and specifically relates to a cold pressing die and a cap-type cold pressing method for aluminum alloy rib web structure forgings. Background Art

[0002] With the development of large-scale and lightweight aerospace structural parts, the large-scale application of aluminum alloys has become an inevitable trend. 7xxx series aluminum alloys are widely used in the aviation field due to their good comprehensive properties such as high strength and corrosion resistance. The aluminum alloy needs to be solution treated at a high temperature of about 470°C and artificially aged after rapid quenching and cooling to obtain excellent comprehensive mechanical properties. However, solution quenching will lead to a problem, that is, the generation of large quenching residual stress. One of the inevitable consequences of heat-treated precipitation-hardened aluminum alloys is the introduction of high-intensity residual stress. When thick and large components are rapidly cooled and quenched from the solution heat treatment temperature, severe thermal gradients will be generated, and large residual stresses with a distribution of "external pressure and internal tension" will be generated after quenching. Due to large quenching residual stress or uneven residual stress, large forgings will have significant processing deformation problems during the processing and manufacturing of large aircraft, making it impossible for parts to achieve the required accuracy and reducing the fatigue life of parts during service. Therefore, controlling residual stress is very critical for 7xxx series aluminum alloys. Cold pressing of aluminum alloy die forgings after solution quenching is one of the main means to control residual stress. Traditional cold pressing methods such as Figure 2 As shown, the cold pressing die includes a rib cold pressing part 21 corresponding to the rib and a web cold pressing part 22 corresponding to the web; the rib cold pressing part 21 is a cavity surrounded by cold pressing side walls 211 on both sides and a cold pressing top wall 212; during cold pressing, the cold pressing top wall 212 cold presses the rib top while the web cold pressing part 22 cold presses the web. It has the following disadvantages:

[0003] First, when the ribs are high, there is a problem that the ribs cannot be pressed through;

[0004] Second, the residual tensile stress in the junction area between the web and the ribs is relatively large. Summary of the invention

[0005] The purpose of the present invention is to provide a cap-type cold pressing method for aluminum alloy rib web structure forgings to reduce residual stress.

[0006] The technical scheme adopted by the present invention is: a cold pressing die for an aluminum alloy rib web structure forging, wherein the aluminum alloy rib web structure forging is a 7xxx series Al-Zn-Mg-Cu aluminum alloy forging; the forging is 500mm-6000mm long and 500mm-4000mm wide; the forging comprises a web and a rib; the forging comprises a rib cold pressing portion corresponding to the rib and a web cold pressing portion corresponding to the web; the rib cold pressing portion is a cavity formed by being surrounded by cold pressing side walls on both sides and a cold pressing top wall, and a cold pressing fillet is arranged between the cold pressing side wall and the cold pressing top wall; the side wall of the rib has a draft angle, and a rib fillet is arranged between the rib top of the rib and the rib side wall; when the rib top is cold pressed by the cold pressing top wall, there is a gap D between the web cold pressing portion and the web of the forging, and D is a gap of 5-15mm; there is a negative gap between the cold pressing fillet of the rib cold pressing portion and the rib fillet, and the cold pressing fillet of the rib cold pressing portion cold presses the rib fillet.

[0007] Furthermore, the negative gap between the cold-pressed fillet of the cold-pressed rib portion and the cold-pressed rib fillet is 0 to -3 mm.

[0008] Furthermore, there is a gap W between the cold-pressed portion of the rib and the rib along the width direction, where W=0-5 mm.

[0009] A method for cold pressing aluminum alloy rib web structure forgings with caps, comprising the following steps:

[0010] Step 1, forging design: according to the structural characteristics of the parts, determine the forging allowance and draft angle, the width of the ribs of the forging is 30mm to 60mm, and the aspect ratio of the ribs is 1 to 5;

[0011] Step 2: designing and manufacturing the cold pressing mold;

[0012] Step 3: After the solution quenching treatment, the aluminum alloy forging is subjected to overall cold compression using a cold pressing die. During overall cold shrinkage, the rib cold pressing part of the cold pressing die simultaneously cold presses the rib top and the rib fillet of the rib. There is a gap between the web cold pressing part and the web, and the web cold pressing part does not cold press the web.

[0013] Furthermore, the cold pressing amount of the rib is t, t=(1%-5%)H, wherein H is the height of the rib.

[0014] Furthermore, the cold pressing speed is 0.2 to 1 mm / s.

[0015] Furthermore, the underpressure value during cold pressing is consistent with the underpressure value of the forging.

[0016] The beneficial effects of the present invention are as follows: the capped cold pressing method for aluminum alloy rib web structure forgings disclosed in the present invention can press the ribs of the aluminum alloy forgings through only by pressing the ribs but not the webs, and the cold pressing amount is relatively uniform, while achieving a better residual stress elimination effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the cross section of aluminum alloy rib web structure forgings;

[0018] Figure 2 This is a schematic diagram of the traditional cold pressing principle;

[0019] Figure 3 It is a schematic diagram of the cold pressing mold of the present invention;

[0020] Figure 4 It is a schematic diagram of the cold pressing principle of the present invention;

[0021] Figure 5 for Figure 4 A partial enlarged view of point A.

[0022] In the figure, the forging 1, the web 11, the rib 12, the rib fillet 121, the cold pressing die 2, the rib cold pressing part 21, the cold pressing side wall 211, the cold pressing top wall 212, the cold pressing fillet 213, and the web cold pressing part 22. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0024] Cold pressing dies for aluminum alloy rib web structure forgings, such as Figure 1 , Figure 3 and Figure 5 As shown, the aluminum alloy rib web structure forging 1 is a 7xxx series Al-Zn-Mg-Cu aluminum alloy forging; the forging 1 is 500mm to 6000mm long and 500mm to 4000mm wide; the forging 1 includes a web 11 and a rib 12; the rib cold-pressed portion 21 corresponding to the rib 12 and the web cold-pressed portion 22 corresponding to the web 11; the rib cold-pressed portion 21 is a cavity formed by surrounding cold-pressed side walls 211 on both sides and a cold-pressed top wall 212, and the cold-pressed side walls 211 and the cold-pressed top wall 212 are connected to each other. A cold-pressed fillet 213 is arranged between the top wall 212; the side wall of the rib 12 has a draft angle, and a rib fillet 121 is arranged between the rib top and the rib side wall of the rib 12; when the cold-pressed top wall 212 cold-presses the rib top of the rib 12, there is a gap D between the cold-pressed web portion 22 and the web 11 of the forging 1, and D=5~15mm gap; there is a negative gap between the cold-pressed fillet 213 of the cold-pressed rib portion 21 and the rib fillet 121, and the cold-pressed fillet 213 of the cold-pressed rib portion 21 cold-presses the rib fillet 121.

[0025] With the cold pressing die of this structure, when the forging 1 is cold pressed, the rib cold pressing portion 21 cold presses the rib top and the rib fillet 121 of the rib 12, which is equivalent to putting a hat on the head of the rib 12, and only presses the rib 12 of the forging 1. Since there is a gap D between the web cold pressing portion 22 and the web 11 of the forging 1, the web 11 of the forging 1 is not directly cold pressed by the web cold pressing portion 22, thereby improving the cold pressing effect of the rib 12 and effectively avoiding the problem of the rib 12 not being pressed through. Similarly, the interface area between the rib 12 and the web 11 is mainly affected by the cold pressing of the rib 12, but not by the cold pressing of the web 11, thereby reducing the residual tensile stress in the interface area between the web 11 and the rib 12. Moreover, during cold pressing, not only the cold pressed top wall 212 of the rib cold pressed portion 21 cold presses the rib top of the rib 12, but the rib cold pressed portion 21 also cold presses the rib fillet 121 of the rib 12, so that the rib cold pressed portion 21 and the rib 12 have a sufficiently large cold pressed contact surface, so that the cold pressing amount of the rib 12 of the aluminum alloy forging is relatively uniform and has a better residual stress elimination effect.

[0026] In order to more effectively cold press the rib 12, press through the rib 12, and make the rib 12 cold pressed uniformly, preferably, the negative gap between the cold pressed fillet 213 of the rib cold pressed portion 21 and the cold pressed rib fillet 121 is 0 to -3 mm.

[0027] A method for cold pressing aluminum alloy rib web structure forgings with caps, comprising the following steps:

[0028] Step 1, design of forging 1: according to the structural characteristics of the part, determine the forging allowance and draft angle, the width of the rib 12 of the forging 1 is 30 mm to 60 mm, and the aspect ratio of the rib is 1 to 5;

[0029] Step 2: designing and manufacturing the cold pressing mold 2;

[0030] Step 3: Figure 4 As shown, the aluminum alloy forging 1 after solution quenching treatment is subjected to overall cold compression by a cold pressing die 2. During overall cold shrinkage, the rib cold pressing portion 21 of the cold pressing die 2 simultaneously cold presses the rib top and the rib fillet 121 of the rib 12. There is a gap between the web cold pressing portion 22 and the web 11, and the web cold pressing portion 22 does not cold press the web 11.

[0031] Preferably, the cold pressing amount of the rib is t, t=(1%-5%)H, wherein H is the height of the rib 12 .

[0032] Preferably, the cold pressing speed is 0.2 to 1 mm / s.

[0033] Preferably, the underpressure value during cold pressing is consistent with the underpressure value of the forging.

[0034] Example:

[0035] The method disclosed in the present invention is used to cold press a forging, the material of the forging is 7050. The specific operation process is as follows:

[0036] Step 1, forging 1 design:

[0037] First of all, according to the structural characteristics of the part, the forging is designed as a bisected mold. On the basis of the part, the machining allowance is increased according to the shape, 10 to 15 mm on one side, and the designed draft angle is 5° to make the forging smoothly demolded. The outer contour dimensions of the forging are 4500mm×1650mm×225mm, the horizontal net projection area is 5.28m2, the web is 1145mm, the ribs are 12 with an aspect ratio of 3.5, and the weight of the forging is 1220Kg.

[0038] Step 2: Design the cold pressing mold 2 and manufacture the mold.

[0039] The rib radius of the cold pressing die of the present invention is less than or equal to the rib radius of the forging, the rib width is slightly larger by 0 to 5 mm, and there is a gap D between the cold pressed web portion 22 and the web 11 of the forging 1, where D=10 mm.

[0040] Step 3: After solution quenching, the aluminum alloy die forgings are subjected to overall cold compression.

[0041] During the cold pressing process, only the ribs 12 are pressed, and the webs 11 are not pressed. The cold pressing amount of the ribs 12 is controlled within 1% to 5% of the height of the ribs 12. The pressing speed is 0.2 to 1 mm / s, the underpressure of the forging is 6 mm, and the underpressure during cold pressing is also controlled to be 6 mm.

[0042] Comparative Example:

[0043] The same forging as in the embodiment was cold pressed using the conventional method mentioned in the background art.

[0044] Table 1 below is a comparison table of mechanical properties and residual stress of comparative examples and embodiments.

[0045] Table 1 Mechanical properties and residual stress

[0046]

[0047] It can be seen from Table 1 that the mechanical properties of the cold forgings obtained in the comparative example and the example are comparable, but the residual stress of the example is significantly reduced, by nearly 50%.

[0048] Attached Figure 1-Figure 4 In the figure, the red dashed line indicates the cold pressing die outline.

[0049] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A cold pressing die for an aluminum alloy rib web structure forging, wherein the aluminum alloy rib web structure forging (1) is a 7xxx series Al-Zn-Mg-Cu aluminum alloy forging; the forging (1) is 500 mm to 6000 mm long and 500 mm to 4000 mm wide; the forging (1) comprises a web (11) and ribs (12); Features: The invention comprises a rib cold-pressed portion (21) corresponding to the rib (12) and a web cold-pressed portion (22) corresponding to the web (11); the rib cold-pressed portion (21) is a cavity formed by being surrounded by cold-pressed side walls (211) on both sides and a cold-pressed top wall (212); a cold-pressed fillet (213) is provided between the cold-pressed side walls (211) and the cold-pressed top wall (212); the side walls of the rib (12) have a draft angle, and the rib top of the rib (12) and the rib side walls are in contact with each other. A rib fillet (121) is arranged between the cold pressed top wall (212) and the rib top of the cold pressed rib (12), a gap D exists between the cold pressed web portion (22) and the web (11) of the forging (1), and D=5-15 mm gap; a negative gap exists between the cold pressed fillet (213) of the cold pressed rib portion (21) and the rib fillet (121), and the cold pressed fillet (213) of the cold pressed rib portion (21) is cold pressed by the rib fillet (121).

2. The cold pressing die for aluminum alloy rib web structure forgings according to claim 1, Features: The negative gap between the cold pressed fillet (213) of the cold pressed rib portion (21) and the cold pressed rib fillet (121) is 0 to -3 mm.

3. The cold pressing die for aluminum alloy rib web structure forgings according to claim 2, Features: There is a gap W between the rib cold-pressed portion (21) and the rib (12) along the width direction, where W=0-5 mm.

4. Aluminum alloy rib web structure forgings with cap-type cold pressing method, Features: The following steps are involved: Step 1, forging (1) design: according to the structural characteristics of the parts, the forging allowance and the draft angle are determined, the width of the rib (12) of the forging (1) is 30 mm to 60 mm, and the aspect ratio of the rib is 1 to 5; Step 2: designing and manufacturing a cold pressing mold (2) as described in any one of claims 1 to 3; Step 3: The aluminum alloy forging (1) after solution quenching treatment is subjected to overall cold compression using a cold pressing die (2). During overall cold shrinkage, the rib cold pressing portion (21) of the cold pressing die (2) simultaneously cold presses the rib top and rib fillet (121) of the rib (12), and there is a gap between the web cold pressing portion (22) and the web (11), and the web cold pressing portion (22) does not cold press the web (11).

5. The hooded cold pressing method for aluminum alloy rib web structure forgings as claimed in claim 4, Features: The cold pressing amount of the rib is t, t=(1%-5%)H, wherein H is the height of the rib (12).

6. The hooded cold pressing method for aluminum alloy rib web structure forgings as claimed in claim 4, Features: The cold pressing speed is 0.2~1mm / s.

7. The hooded cold pressing method for aluminum alloy rib web structure forgings as claimed in claim 6, Features: The underpressure value during cold pressing is consistent with the underpressure value of forgings.

Citation Information

Patent Citations

  • Method for eliminating residual stress after solid dissolution by oversize rib web plate type aluminum alloy die forging

    CN108315674A

  • Method for reducing residual stress of large complex aluminum alloy die forgings

    CN109234653A

  • Die for cold compression, and method for removing residual stress of stamp forging

    JP2003211248A

Cited By

  • Method and die for reducing residual stress of large aluminum alloy whole frame through low-load cold pressing

    CN119609022A

  • Method for eliminating residual stress of aluminum alloy die forging

    CN121538581A