High platform capacity lignin-based hard carbon material as well as preparation method and application thereof

By classifying lignin to remove polar functional groups, lignin-based hard carbon materials with high platform capacity are formed, which solves the problem of low platform capacity of lignin-based hard carbon materials in the existing technology and achieves the energy density of sodium-ion batteries. Improved and environmentally friendly production.

CN118744981AInactive Publication Date: 2024-10-08GUANGDONG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410826606.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to develop lignin-based hard carbon materials with a high platform capacity ratio for sodium-ion battery anodes under the conditions of low cost, simple process and environmental protection with existing technology, resulting in limited energy density of sodium-ion batteries.

Method used

By classifying lignin and organic solvents to remove polar functional groups, a lignin precursor with a larger molecular weight and less polarity is formed, and closed pores are formed during the high-temperature carbonization process to prepare a high platform capacity lignin base Hard carbon material.

Benefits of technology

The lignin-based hard carbon material that achieves high platform capacity and high platform capacity ratio improves the energy density and cycle stability of sodium-ion batteries, simplifies the preparation process, reduces production costs, and is easy to protect the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910677720000151
    Figure BDA0004910677720000151
  • Figure HDA0004910677730000011
    Figure HDA0004910677730000011
  • Figure HDA0004910677730000012
    Figure HDA0004910677730000012
Patent Text Reader

Abstract

The invention discloses a high platform capacity lignin-based hard carbon material as well as a preparation method and application thereof. The method comprises the following steps: carrying out grading treatment on lignin by adopting an organic solvent to obtain lignin components with different molecular weights and different polarities, and carbonizing the lignin components in a protective gas atmosphere to obtain the hard carbon material. The lignin component with large molecular weight and low polar functional group content can be obtained through organic solvent grading, so that the prepared hard carbon material has rich closed pores and large closed pore volume. The hard carbon material shows extremely high platform capacity and good specific capacity, rate capability and cycling stability when applied to a sodium-ion battery negative electrode. The method has the advantages that the operation is simple, the requirement on equipment is low, the used volatile solvent is easy to recover, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a high-platform capacity lignin-based hard carbon material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have an overwhelming advantage in the energy market due to their high energy density, superior cycle performance, and long cycle life. However, the shortage of lithium resources and the uneven distribution of lithium resources cannot meet the rapid growth of society's demand for lithium, which makes it difficult for lithium-ion batteries to be used in large-scale energy storage. Sodium-ion batteries can make up for the shortcomings of lithium-ion batteries in large-scale use due to their abundant sodium reserves and similar chemical properties to lithium.

[0003] At present, hard carbon has been developed as a commercial sodium-ion battery negative electrode material. The sodium storage behavior of hard carbon includes high-potential slope behavior and low-potential platform behavior. The size of the slope capacity (>0.1V) is determined by the number of functional groups and the richness of defects, which usually brings many irreversible sodium ion adsorption sites, resulting in low ICE and energy density. The platform capacity (<0.1V) mainly comes from the filling of sodium ions in closed air. The high low-potential platform capacity is conducive to the high output voltage of sodium-ion batteries and can construct high-energy-density sodium-ion batteries. However, about 30% of the capacity of typical hard carbon comes from the high-potential slope area. Even through high-temperature carbonization, it is difficult to reduce the oxygen content and defect content in hard carbon, which limits the energy density of sodium-ion batteries. Therefore, the development of a hard carbon negative electrode with a high platform capacity ratio is the key to improving the energy density of sodium-ion batteries.

[0004] Increasing the number of closed nanopores in the hard carbon anode is conducive to achieving high platform capacity sodium ion storage. The literature (Advanced Energy Materias 2019, 9, 1902852) selected discarded cork as a precursor and designed a series of hard carbon materials through a simple pre-oxidation treatment and high-temperature calcination steps. Increasing the pyrolysis temperature to reduce open pores and increase closed pores, which increased its platform capacity from 160mAh·g -1 Significantly increased to 231mAh·g -1. When the carbonization temperature is 1600°C, the platform capacity accounts for 64%, which makes the energy density of the sodium-ion battery reach 230Wh / kg. However, the pre-oxidation process will introduce more oxygen functional groups and defects, resulting in an increase in the slope capacity, which is not conducive to increasing the platform capacity ratio. The literature (AdvancedEnergy Materials 2024, 14, 2303064) developed a strategy for CO2 etching and carbonization using starch as a precursor, which can induce a large number of closed nanopores to store sodium ions. This method activates and etches starch with CO2 at a relatively low temperature (800°C), which will produce a large number of open pores. Subsequently, after high-temperature carbonization at 1300°C, the open pores are converted into closed pores to achieve high-performance sodium storage. The starch-based hard carbon material synthesized by this method has an extremely high platform capacity of 351mAh·g -1 , accounting for 72% of the total capacity. The high platform capacity makes the full battery prepared by it have 281Wh·kg -1 This shows that the high platform capacity ratio can improve the energy density of sodium-ion batteries. However, this method has a large loss of equipment in the long term, high energy consumption of two-step carbonization, and high production cost, which is not conducive to large-scale industrial production.

[0005] Chinese patent application CN115974045A discloses a method for preparing hard carbon materials by chemical gelation and alkaline metal oxide template method and its application. The invention heats the polysaccharide and alkaline metal salt solution to form a sol and gel state, freezes and freeze-dries it, and then pyrolyzes it to generate granular alkaline metal oxide inside the carbon material, then removes the alkaline metal oxide particles through acid treatment, and finally obtains the hard carbon material through a high-temperature carbonization step. The hard carbon material prepared by the invention has a high thermal conductivity of up to 393 mA·hg -1 The platform capacity accounts for 82%. However, this method has a complex production process and produces acid and alkali waste liquid, which has the characteristics of high production cost and unfriendly environment, and is not conducive to large-scale industrial production.

[0006] Chinese patent application CN117466278A discloses a method of obtaining a ball-milled modified hard carbon material by simply ball-milling a hard carbon material. The invention adjusts the ball-to-material ratio and the ball-milling intensity to control the pore structure, thereby adjusting the low-potential platform capacity ratio (capacity below 0.2V) of the hard carbon. The invention has a simple process, but the hard carbon material prepared by it is used as the negative electrode of a sodium ion battery, and the low-potential platform capacity ratio is only up to 60%, and the platform capacity ratio is still low.

[0007] The above-mentioned method for preparing hard carbon materials with high platform capacity ratio is difficult to simultaneously take into account the industrial production indicators such as low cost, simple production process, and environmental friendliness. Lignin, as a by-product of cellulosic ethanol and traditional papermaking industry, has the advantages of being green, environmentally friendly, and sustainable. It is an ideal precursor for preparing hard carbon negative electrodes for sodium ion batteries. However, hard carbon materials prepared directly from industrial lignin have a lower platform capacity of about 120 to 200 mAh g -1 (Carbon Res. 2024; 3: 28.). At present, there is a lack of research on the use of lignin as a carbon source to prepare hard carbon materials with a high platform capacity ratio. The complexity and diversity of lignin functional groups easily lead to different microstructures of the prepared hard carbon. Therefore, it is necessary to develop a low-cost, simple process, and environmentally friendly pretreatment method to prepare lignin-based hard carbon materials with a high platform capacity ratio by regulating the functional groups in lignin to form a microstructure suitable for sodium storage. Summary of the invention

[0008] In view of the problem that the hard carbon materials prepared from existing industrial lignin have a low platform capacity ratio, and the existing pretreatment technology for improving the platform capacity of lignin is difficult to take into account important industrialization indicators such as low cost, simple preparation route and green environmental protection, the primary purpose of the present invention is to propose a preparation method of high platform capacity lignin-based hard carbon materials, specifically, directly carbonizing lignin treated with organic solvents to prepare hard carbon materials.

[0009] The present invention can prepare a lignin precursor with a large molecular weight and a low content of polar functional groups through simple operations. At the same time, the organic solvent used is volatile, and the goal of saving raw materials and protecting the environment can be achieved through condensation recovery. The lignin precursor is used to prepare the negative electrode material of sodium ion batteries. Lignin with fewer polar functional groups is more likely to form closed pores during high-temperature carbonization, which makes the prepared lignin-based hard carbon material have extremely high platform capacity and high platform capacity ratio.

[0010] Another object of the present invention is to provide a high platform capacity lignin-based hard carbon material prepared by the above preparation method.

[0011] Another object of the present invention is to provide the use of the above-mentioned high platform capacity lignin-based hard carbon material as a negative electrode material for sodium ion batteries.

[0012] The purpose of the present invention is achieved through the following technical solutions:

[0013] A method for preparing a high platform capacity lignin-based hard carbon material comprises the following steps:

[0014] (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1;

[0015] (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2;

[0016] Refer to step (2) and repeat the following steps 1 to 5 times:

[0017] (n) mixing and dissolving the insoluble solid obtained in the previous step with an organic solvent, separating the solid and the liquid to obtain a mixed solution n and an insoluble solid n, and removing the organic solvent from the mixed solution n to obtain a soluble lignin component n;

[0018] (n+1) carbonizing at least one of the insoluble solids obtained in the above steps (1) to (n) and / or at least one of the soluble lignin components obtained in the above steps (2) to (n) under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material;

[0019] Where n is 3 to 7.

[0020] Preferably, the method for preparing the high platform capacity lignin-based hard carbon material comprises the following steps:

[0021] (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1;

[0022] (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2;

[0023] (3) mixing and dissolving the insoluble solid 2 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 3 and an insoluble solid 3, and removing the organic solvent from the mixed solution 3 to obtain a soluble lignin component 3;

[0024] (4) mixing and dissolving the insoluble solid 3 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 4 and an insoluble solid 4, and removing the organic solvent from the mixed solution 4 to obtain a soluble lignin component 4;

[0025] (5) Carbonizing at least one of the insoluble solid 1, insoluble solid 2, insoluble solid 3, insoluble solid 4, soluble lignin component 2, soluble lignin component 3 and soluble lignin component 4 under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

[0026] Preferably, the method for preparing the high platform capacity lignin-based hard carbon material comprises the following steps:

[0027] (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1;

[0028] (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2;

[0029] (3) mixing and dissolving the insoluble solid 2 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 3 and an insoluble solid 3, and removing the organic solvent from the mixed solution 3 to obtain a soluble lignin component 3;

[0030] (4) Carbonizing at least one of the insoluble solid 1, the insoluble solid 2, the insoluble solid 3, the soluble lignin component 2 and the soluble lignin component 3 under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

[0031] Preferably, the lignin in step (1) is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, alkali lignin extracted from black liquor of alkali pulping, and lignin sulfonate.

[0032] Preferably, the organic solvent in steps (1) to (n) is at least one of methanol, ethanol, acetone and ethyl acetate, wherein n is 3 to 7; more preferably, the organic solvent in steps (1) to (n) is one of methanol, ethanol, acetone and ethyl acetate, and the organic solvent in each step is different; most preferably, the organic solvent in steps (1) to (n) is one of methanol, ethanol, acetone and ethyl acetate, and the polarity of the organic solvent gradually decreases from large to small, wherein the polarity is: methanol>ethanol>acetone>ethyl acetate.

[0033] Preferably, the ratio of lignin to organic solvent in step (1) is 1 g: (5-25) mL; more preferably 1 g: (10-25) mL; the ratio of insoluble solid to organic solvent in steps (2) to (n) is 1 g: (10-20) mL, wherein n is 3-7.

[0034] Preferably, the mixed solution in steps (1) to (n) is subjected to rotary evaporation or volatilization to remove the organic solvent to obtain a soluble lignin component, wherein n is 3 to 7.

[0035] Preferably, the solid-liquid separation method in steps (1) to (n) is filtration, wherein n is 3 to 7.

[0036] Preferably, the protective gas in step (n+1) is at least one of nitrogen, argon and helium, wherein n is 3-7.

[0037] Preferably, the insoluble solids in steps (1) to (n) and the soluble lignin components in steps (1) to (n) need to be dried at a temperature of 40 to 120° C. for 2 to 24 hours; more preferably, the drying temperature is 60 to 80° C. for 6 to 14 hours.

[0038] Preferably, the time for the mixed dissolution in steps (1) to (n) is 2 to 24 hours.

[0039] Preferably, the carbonization temperature in step (n+1) is 1000-1600° C., and the time is 2-6 h; more preferably, the carbonization temperature is 1100-1600° C., and the time is 2-6 h, wherein n is 3-7.

[0040] Preferably, the heating rate of the carbonization in step (n+1) is 1-10°C / min, more preferably 5°C / min; the flow rate of the protective gas is 40-80mL / min, more preferably 60mL / min.

[0041] In a preferred embodiment of the present invention, the method for preparing the high platform capacity lignin-based hard carbon material comprises the following steps:

[0042] (1) mixing lignin with an organic solvent and dissolving it, separating the solid and the liquid to obtain an insoluble solid;

[0043] (2) The insoluble solid is carbonized under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

[0044] In a preferred embodiment of the present invention, the method for preparing the high platform capacity lignin-based hard carbon material comprises the following steps:

[0045] (1) mixing and dissolving lignin with an organic solvent, separating the solid and the liquid, and obtaining an insoluble solid;

[0046] (2) mixing and dissolving the insoluble solid with the organic solvent, separating the solid and the liquid to obtain a mixed solution, and removing the organic solvent from the mixed solution to obtain a soluble lignin component;

[0047] (3) The soluble lignin component is carbonized under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

[0048] In a preferred embodiment of the present invention, the method for preparing the high platform capacity lignin-based hard carbon material comprises the following steps:

[0049] (1) mixing lignin with an organic solvent and dissolving it, separating the solid and the liquid to obtain an insoluble solid;

[0050] (2) mixing and dissolving the insoluble solid obtained in step (1) with an organic solvent, and separating the solid from the liquid to obtain an insoluble solid;

[0051] (3) mixing and dissolving the insoluble solid from step (2) with an organic solvent, separating the solid and the liquid to obtain a mixed solution, and removing the organic solvent from the mixed solution to obtain a soluble lignin component;

[0052] (4) The soluble lignin component is carbonized under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

[0053] The preparation method comprises the following steps (1) to (n): subjecting lignin to continuous graded treatment with organic solvents of gradually decreasing polarity, thereby obtaining different lignin components, wherein the lignin components have different molecular weights and polar functional group contents, wherein the molecular weight gradually increases and the molecular polarity gradually decreases, and the lignin components with larger molecular weight and more moderate polarity are used to prepare hard carbon materials.

[0054] The high platform capacity lignin-based hard carbon material prepared by the above preparation method.

[0055] The above-mentioned high platform capacity lignin-based hard carbon material is used as a negative electrode material for sodium ion batteries.

[0056] The high-platform capacity lignin-based hard carbon material of the present invention is used to prepare a negative electrode for a sodium ion battery: the lignin-based hard carbon material, acetylene black conductive agent, and polyvinylidene fluoride (PVDF) binder are weighed in a mass ratio of 8:1:1 respectively, PVDF is dissolved in an appropriate amount of 1-methyl-2-pyrrolidone (NMP), and stirred until completely dissolved, and then the evenly ground active material and acetylene black are added to the above solution, and stirring is continued to ensure that the slurry is evenly mixed; then the slurry is evenly coated on a round copper foil (diameter 12 mm), dried in a vacuum oven at 100° C., and finally flattened on a tablet press with a pressure of 10 MPa to obtain an electrode sheet.

[0057] The prepared electrode sheet, sodium sheet and diaphragm were assembled into a CR2025 button-type sodium ion battery in a glove box filled with high-purity argon. The electrolyte was 1 mol / L NaPF6 DME electrolyte, and the battery test system was used to test the charge and discharge performance and cycle stability of the sodium ion battery.

[0058] The specific surface area of ​​the high platform capacity lignin-based hard carbon material of the present invention is 5 to 150 m 2 / g, with abundant closed pores and large closed pore volume; sodium ion half-cells were assembled in 1 mol / L NaPF6DME electrolyte, and the sodium ion battery showed an extremely high platform capacity of 200-250 mAh·g -1 , and a high platform capacity share of more than 70%, reflecting excellent rate performance and cycle stability.

[0059] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0060] (1) The present invention constructs a precursor through a lignin classification method, dissolves lignin in an organic solvent to achieve classification, and can prepare a lignin precursor with a high molecular weight and a low polar functional group content. The lignin precursor is carbonized in one step to obtain a hard carbon material. The preparation process is simple and does not require heating reaction and other complicated pretreatment steps. At the same time, the organic solvent used in the present invention is volatile and can be recovered by condensation reflux, solving the environmental pollution problem of excess organic solvents. Therefore, the present invention has the advantages of simple preparation process, low cost and resource friendliness.

[0061] (2) The lignin precursor prepared by the present invention has a low content of polar functional groups, so that the lignin precursor generates more micropores during low-temperature pyrolysis, which is conducive to the formation of closed pores during high-temperature carbonization. The organic solvent used is volatile and is removed at low temperatures, and no impurities are generated without washing, which reduces the purification cost in the process of preparing hard carbon and is conducive to large-scale production.

[0062] (3) The hard carbon material prepared by the lignin fractionation method of the present invention has abundant closed pores and large closed pore volume. Abundant closed pores and large pore volume can improve the sodium storage performance in the low potential plateau. Therefore, the hard carbon negative electrode material prepared by the lignin fractionation method has an extremely high platform capacity and good reversible specific capacity, rate performance and cycle stability, and this hard carbon material is conducive to commercial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 Example 1: The lignin-based hard carbon material (1-EA-R-1300) is used as the negative electrode of the sodium ion battery at 0.05 A·g -1 The second cycle charge and discharge curve under current density.

[0064] Figure 2 This is a graph showing the change in specific capacitance of the lignin-based hard carbon material (1-EA-R-1300) used as the negative electrode of a sodium ion battery in Example 1 as a function of current density.

[0065] Figure 3 This is the nitrogen adsorption-desorption isotherm of the lignin-based hard carbon material (2-A-1300) of Example 4.

[0066] Figure 4 This is the pore size distribution diagram of the lignin-based hard carbon material (2-A-1300) of Example 4.

[0067] Figure 5 This is the SAXS graph of the lignin-based hard carbon material (2-A-1300) of Example 4.

[0068] Figure 6Example 4: The lignin-based hard carbon material (2-A-1300) is used as the negative electrode of the sodium ion battery at 0.05 A·g -1 The second cycle charge and discharge curve under current density.

[0069] Figure 7 Comparative Example 1: Lignin-based hard carbon material (1-EA-1300) is used as a negative electrode for sodium ion batteries at 0.05 A·g -1 The second cycle charge and discharge curve under current density.

[0070] Figure 8 This is a graph showing the change in specific capacitance with current density of the lignin-based hard carbon material (1-EA-1300) used as the negative electrode of a sodium ion battery in Comparative Example 1. DETAILED DESCRIPTION

[0071] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0072] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.

[0073] Example 1

[0074] (1) Add 10 g of alkali lignin into 100 mL of ethyl acetate and stir at room temperature for 2.5 h to obtain a suspension.

[0075] (2) filtering the suspension in step (1) to obtain a filtrate and a filter residue.

[0076] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent, thereby obtaining a lignin component soluble in ethyl acetate.

[0077] (4) Drying the filter residue from step (2) at 70° C. for 12 h to obtain a one-step fractionated lignin component insoluble in ethyl acetate, named 1-EA-R.

[0078] (5) The 1-EA-R in step (4) was heated to 1300°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min, and pyrolyzed and carbonized for 4 h to obtain a hard carbon material named 1-EA-R-1300.

[0079] (6) 1-EA-R-1300, conductive carbon black and PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 8:1:1, and ultrapure water was added and stirred to prepare a slurry of sodium ion battery electrode material. The slurry was applied on a copper foil with a thickness of 150 μm, and finally, it was dried and rolled and cut into round electrode sheets with a diameter of 14 mm for standby use.

[0080] The prepared sodium ion battery electrode sheet was used as the working electrode, the sodium metal sheet as the counter electrode, and 1 mol / LNaPF6 (DME as the solvent) as the electrolyte to assemble a sodium ion half-cell, and the sodium ion storage performance of 1-EA-R-1300 was tested, wherein DME was ethylene glycol dimethyl ether.

[0081] Figure 1 1-EA-R-1300 is used as the negative electrode of sodium ion battery at 0.05A·g -1 The second cycle charge and discharge curve under current density. At 0.05A·g -1 At a current density of 1.34 W, the platform capacity of 1-EA-R-1300 in the second cycle is as high as 250 mAh g -1 , the platform capacity accounts for 72%.

[0082] Figure 2 This is a graph showing the change of specific capacitance with current density when the lignin-based hard carbon material (1-EA-R-1300) is used as the negative electrode of a sodium ion battery in Example 1. -1 At a current density of 348 mAh g -1 The specific capacity at 5A·g -1 At a current density of 142 mAh g -1 This indicates that 1-EA-R-1300 has good rate performance when used as the negative electrode of sodium ion batteries.

[0083] Example 2

[0084] (1) Add 5 g of enzymatically hydrolyzed lignin into 100 mL of acetone and stir at room temperature for 2 h to obtain a suspension.

[0085] (2) filtering the suspension in step (1) to obtain a filtrate and a filter residue.

[0086] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent and obtain a soluble lignin component.

[0087] (4) Drying the filter residue from step (2) at 60° C. for 14 h to obtain an acetone-insoluble lignin component that has been fractionated in one step and named 1-AR.

[0088] (5) The 1-AR in step (4) was heated to 1100°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and pyrolyzed and carbonized for 6 h to obtain a hard carbon material named 1-AR-1100.

[0089] Example 3

[0090] (1) 50 g of alkali lignin was placed in 800 mL of ethanol and stirred at room temperature for 24 h to obtain a suspension.

[0091] (2) filtering the suspension in step (1) to obtain a filtrate and a filter residue.

[0092] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent and obtain a soluble lignin component.

[0093] (4) Drying the filter residue from step (2) at 80° C. for 6 h to obtain an ethanol-insoluble lignin component that has been fractionated in one step and named 1-ER.

[0094] (5) The 1-ER prepared in step (4) was heated to 1500°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min and pyrolyzed and carbonized for 2 h to obtain a hard carbon material named 1-ER-1500.

[0095] Example 4

[0096] (1) 20 g of alkali lignin was added to 500 mL of ethanol and stirred at room temperature for 12 h to obtain suspension 1.

[0097] (2) Filter the suspension 1 in step (1) to obtain a filtrate 1 and a filter residue 1.

[0098] (3) After drying the filter residue obtained in step (2) at 80°C for 6 h, 10 g of the filter residue was added to 200 mL of acetone and stirred at room temperature for 12 h to obtain suspension 2.

[0099] (4) Filter the suspension 2 obtained in step (3) to obtain a filtrate 2 and a filter residue 2.

[0100] (5) The filtrate 2 obtained in step (4) is subjected to rotary evaporation to recover the solvent, thereby obtaining a twice-graded acetone-soluble lignin component, which is named 2-A.

[0101] (6) 2-A in step (5) was heated to 1300°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min, and pyrolyzed and carbonized for 6 h to obtain a hard carbon material named 2-A-1300.

[0102] The nitrogen adsorption and desorption isotherm and pore size distribution of 2-A-1300 hard carbon negative electrode material are shown in the figure. Figure 3 and Figure 4 shown. Figure 3 The increase in nitrogen adsorption in the low adsorption pressure region indicates the presence of micropores, while a significant increase in nitrogen adsorption occurs at high adsorption pressure, indicating the presence of mesopores. Figure 4 The pore size distribution diagram also verifies this conclusion.

[0103] Small angle X-ray scattering diagram of 2-A-1300 hard carbon negative electrode material Figure 5 As shown. Figure 5 0.05A can be observed -1 Up to 0.4A -1 There is an obvious shoulder peak in the range of 0.25 cm 3 / g) and a large average closed-cell pore size (1.98 nm).

[0104] 2-A-1300, conductive carbon black and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 8:1:1, stirred evenly and coated on copper foil, which was dried and rolled and cut into circular electrode sheets with a diameter of 12 mm for standby use. The prepared electrode sheet was used as the working electrode, the sodium metal sheet was used as the counter electrode, and 1 mol / L NaPF6 (DME as solvent) was used as the electrolyte to assemble a sodium ion half-cell to test the sodium ion storage performance of 2-A-1300, where DME is ethylene glycol dimethyl ether.

[0105] Figure 6 In Example 4, 2-A-1300 is used as the negative electrode of the sodium ion battery. -1 The second cycle charge and discharge curve under current density. At 0.05A·g -1 At a current density of 2.5, the platform capacity of 2-A-1300 in the second cycle is 244 mAh g -1 , at this time, the platform capacity accounts for as much as 78%, which is attributed to the large number of closed pores and large closed pore volume.

[0106] Example 5

[0107] (1) 30 g of alkali lignin was added to 600 mL of ethanol and stirred at room temperature for 16 h to obtain suspension 1.

[0108] (2) Filter the suspension 1 in step (1) to obtain a filtrate 1 and a filter residue 1.

[0109] (3) After drying the filter residue 1 obtained in step (2) at 70° C. for 12 h, 20 g of the filter residue 1 was added to 200 mL of ethyl acetate and stirred at room temperature for 16 h to obtain a suspension 2.

[0110] (4) Filter the suspension 2 obtained in step (3) to obtain a filtrate 2 and a filter residue 2.

[0111] (5) The filtrate 2 obtained in step (4) is subjected to rotary evaporation to recover the solvent, thereby obtaining a lignin component soluble in ethyl acetate after two classifications, which is named 2-EA.

[0112] (6) The 2-EA in step (5) was pyrolyzed and carbonized at 1400°C for 4 h at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain a hard carbon material named 2-EA-1400.

[0113] Example 6

[0114] (1) 40 g of enzymatically hydrolyzed lignin was added to 800 mL of ethanol and stirred at room temperature for 24 h to obtain suspension 1.

[0115] (2) Filter the suspension 1 in step (1) to obtain a filtrate 1 and a filter residue 1.

[0116] (3) After drying the filter residue 1 obtained in step (2) at 80° C. for 10 h, 30 g of the filter residue 1 was added to 600 mL of acetone and stirred at room temperature for 24 h to obtain a suspension 2.

[0117] (4) Filter the suspension 2 obtained in step (3) to obtain a filtrate 2 and a filter residue 2.

[0118] (5) After drying the filter residue 2 obtained in step (4) at 80° C. for 10 h, 20 g of the filter residue 2 was added to 400 mL of ethyl acetate and stirred at room temperature for 24 h to obtain a suspension 3.

[0119] (6) The suspension 3 obtained in step (5) is filtered to obtain a filter residue 3 and a filtrate 3.

[0120] (7) The filtrate 3 obtained in step (6) is subjected to rotary evaporation to recover the solvent, thereby obtaining a lignin component soluble in ethyl acetate after three-stage classification, which is named 3-EA.

[0121] (8) The 3-EA in step (7) was pyrolyzed and carbonized at 1600°C for 2 h at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain a hard carbon material named 3-EA-1600.

[0122] Comparative Example 1

[0123] (1) Add 10 g of alkali lignin into 100 mL of ethyl acetate and stir at room temperature for 2.5 h to obtain a suspension.

[0124] (2) filtering the suspension in step (1) to obtain a filtrate and a filter residue.

[0125] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent, thereby obtaining a lignin component soluble in ethyl acetate after a primary classification, which is named 1-EA.

[0126] (4) The 1-EA in step (3) was pyrolyzed and carbonized at 1300°C for 4 h at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min to obtain a hard carbon material named 1-EA-1300.

[0127] (5) 1-EA-1300, carbon black and PVDF were mixed in a mass ratio of 8:1:1, and ultrapure water was added and stirred to prepare a slurry for the negative electrode of the sodium ion battery. The slurry was applied on a copper foil with a thickness of 150 μm, and finally, it was dried and rolled and cut into a round electrode sheet with a diameter of 14 mm for standby use.

[0128] The prepared sodium ion battery electrode sheet was used as the working electrode, the sodium metal sheet as the counter electrode, and 1 mol / LNaPF6 (DME as the solvent) as the electrolyte to assemble a sodium ion half-cell, and the electrochemical properties of 1-EA-1300 were tested.

[0129] Figure 7 Comparative Example 1: The hard carbon material 1-EA-1300 prepared by lignin fractionation is used as the negative electrode of the sodium ion battery. -1 The second cycle charge and discharge curve under current density. At 0.05A·g -1 At a current density of 1.34 W, the platform capacity of 1-EA-1300 in the second cycle was only 181 mAh g -1 , the platform capacity accounts for 65%.

[0130] Figure 8 The hard carbon material (1-EA-1300) prepared by lignin fractionation is used as the negative electrode of sodium ion battery, and its specific capacitance changes with current density. -1 At a current density of 277 mAh g -1 The specific capacity at 5A·g -1 At a current density of 111 mAh g -1 Specific capacity.

[0131] Figure 7 and Figure 8 It shows that 1-EA-1300 with small molecular weight and high polarity has low specific capacity and platform capacity, as well as poor rate performance when used as the negative electrode of sodium ion batteries.

[0132] Comparative Example 2

[0133] (1) Add 5 g of enzymatically hydrolyzed lignin into 100 mL of acetone and stir at room temperature for 2 h to obtain a suspension.

[0134] (2) Filter the suspension obtained in step (1) to obtain a filtrate and a filter residue.

[0135] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent, thereby obtaining a first-classified acetone-soluble lignin component, which is named 1-A.

[0136] (4) 1-A in step (3) was heated to 1100°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min, and pyrolyzed and carbonized for 6 h to obtain a hard carbon material named 1-A-1100.

[0137] Comparative Example 3

[0138] (1) Add 50 g of alkali lignin to 800 mL of ethanol and stir at room temperature for 24 h to obtain a suspension.

[0139] (2) filtering the suspension in step (1) to obtain a filtrate and a filter residue.

[0140] (3) The filtrate obtained in step (2) is subjected to rotary evaporation to recover the solvent, thereby obtaining a lignin component soluble in ethanol after a first classification, which is named 1-E.

[0141] (4) 1-E in step (3) was heated to 1500°C at a heating rate of 5°C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min, and pyrolyzed and carbonized for 2 h to obtain a hard carbon material named 1-E-1500.

[0142] Comparative Example 4

[0143] (1) 2 g of alkali lignin (without any classification treatment) was heated to 1300 °C at a heating rate of 5 °C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min for 4 h to obtain a hard carbon material named AL-1300.

[0144] Comparative Example 5

[0145] (1) Take 2 g of enzymatically hydrolyzed lignin (without any classification treatment) and heat it to 1300 °C at a heating rate of 5 °C / min under a nitrogen atmosphere with a gas flow rate of 60 mL / min for pyrolysis and carbonization for 6 h to obtain a hard carbon material named EHL-1300.

[0146] Table 1 shows the specific surface area, closed pore volume and platform capacity (0.05A·g) of the hard carbon materials prepared in the above examples and the samples prepared in the above comparative examples. -1 ) and other aspects of the comparison.

[0147] Table 1

[0148]

[0149] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a high platform capacity lignin-based hard carbon material, characterized in that: The following steps are involved: (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1; (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2; Refer to step (2) and repeat the following steps 1 to 5 times: (n) mixing and dissolving the insoluble solid obtained in the previous step with an organic solvent, separating the solid and the liquid to obtain a mixed solution n and an insoluble solid n, and removing the organic solvent from the mixed solution n to obtain a soluble lignin component n; (n+1) carbonizing at least one of the insoluble solids obtained in the above steps (1) to (n) and / or at least one of the soluble lignin components obtained in the above steps (2) to (n) under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material; Where n is 3 to 7.

2. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The following steps are involved: (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1; (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2; (3) mixing and dissolving the insoluble solid 2 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 3 and an insoluble solid 3, and removing the organic solvent from the mixed solution 3 to obtain a soluble lignin component 3; (4) mixing and dissolving the insoluble solid 3 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 4 and an insoluble solid 4, and removing the organic solvent from the mixed solution 4 to obtain a soluble lignin component 4; (5) Carbonizing at least one of the insoluble solid 1, insoluble solid 2, insoluble solid 3, insoluble solid 4, soluble lignin component 2, soluble lignin component 3 and soluble lignin component 4 under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

3. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The following steps are involved: (1) mixing and dissolving lignin with an organic solvent, and separating the solid and the liquid to obtain a mixed solution 1 and an insoluble solid 1; (2) mixing and dissolving the insoluble solid 1 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 2 and an insoluble solid 2, and removing the organic solvent from the mixed solution 2 to obtain a soluble lignin component 2; (3) mixing and dissolving the insoluble solid 2 with an organic solvent, separating the solid and the liquid to obtain a mixed solution 3 and an insoluble solid 3, and removing the organic solvent from the mixed solution 3 to obtain a soluble lignin component 3; (4) Carbonizing at least one of the insoluble solid 1, the insoluble solid 2, the insoluble solid 3, the soluble lignin component 2 and the soluble lignin component 3 under a protective gas atmosphere to obtain a high platform capacity lignin-based hard carbon material.

4. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The organic solvent in steps (1) to (n) is at least one of methanol, ethanol, acetone and ethyl acetate; The ratio of lignin to organic solvent in step (1) is 1 g: (5-25) mL; The mass of the insoluble solid and the organic solvent in steps (2) to (n) is 1 g: (10 to 20) mL; The time for the mixed dissolution in steps (1) to (n) is 2 to 24 hours.

5. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The carbonization temperature of step (n+1) is 1000-1600° C. and the time is 2-6 hours; The heating rate of the carbonization in step (n+1) is 1-10°C / min; the flow rate of the protective gas is 40-80mL / min.

6. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The lignin in step (1) is at least one of enzymatic lignin extracted from biorefining residues, organic solvent lignin obtained from solvent pulping, alkali lignin extracted from black liquor of alkali pulping, and lignin sulfonate.

7. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The organic solvent in steps (1) to (n) is one of methanol, ethanol, acetone and ethyl acetate, and the organic solvent in each step is different; The ratio of lignin to organic solvent in step (1) is 1 g: (10-25) mL.

8. The method for preparing a high platform capacity lignin-based hard carbon material according to claim 1, characterized in that: The carbonization temperature of step (n+1) is 1100-1600° C. and the time is 2-6 hours; The organic solvent in steps (1) to (n) is one of methanol, ethanol, acetone and ethyl acetate, and the polarity of the organic solvent in steps (1) to (n) gradually decreases from large to small; The protective gas in step (n+1) is at least one of nitrogen, argon and helium, wherein n is 3 to 7; The insoluble solids in steps (1) to (n) and the soluble lignin components in steps (1) to (n) need to be dried at a temperature of 40 to 120° C. for 2 to 24 hours.

9. A high-platform capacity lignin-based hard carbon material obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the high platform capacity lignin-based hard carbon material according to claim 9 as a negative electrode material for a battery.

Citation Information

Cited By

  • Preparation method for lignin-based binder, and use of lignin-based binder in double-layer supercapacitor

    WO2026103945A1