Self-compacting gypsum concrete backfill leveling material and application thereof
By using self-compacting gypsum concrete backfilling and leveling materials in residential buildings, combined with the proportion of cementitious materials and aggregates, the problems of long construction period and insufficient strength of traditional backfilling and leveling materials are solved, and the effects of efficient construction and high tensile strength are achieved. , suitable for backfilling and leveling in dry areas of residential buildings.
Patent Information
- Application Number
- CN202410732585.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
The ground backfilling and leveling materials of traditional residential buildings have problems such as long construction period, hollowing, cracking, and sanding of the ground. In addition, the thermal conductivity of the floor heating system in the southern region is insufficient, and lightweight concrete and foamed gypsum are not sufficient in terms of functionality and strength. demand, resulting in limited application in residential buildings.
Self-compacting gypsum concrete backfill leveling material is used. By introducing a special cementitious material system and well-matched coarse and fine aggregates, the elastic modulus and compactness of the material are increased, the tensile strength is improved, and construction pumping is taken into consideration. Improve material stability and construction efficiency.
It achieves efficient construction, good material system stability, and high tensile strength backfill leveling layer, which is suitable for flooring and ceramic tile paving. It solves the shortcomings of traditional materials in strength and thermal conductivity, and is suitable for dry areas of residential buildings. Backfill screed.
Smart Images

Figure BDA0004881034630000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of building materials, and in particular to a self-compacting gypsum concrete backfill leveling material and a use thereof. Background Art
[0002] The traditional method of backfilling and leveling materials for residential buildings is mainly fine stone concrete, supplemented by cement floor mortar. The construction period is long, and problems such as floor hollowing, cracking, and sanding have become stubborn problems. As the floor adds energy-saving and heat-insulating functions, the heat transfer coefficient decreases, and lightweight concrete and lightweight mortar begin to be promoted. With the gradual reduction of ceramsite, lightweight concrete becomes foamed cement, and lightweight mortar becomes foamed gypsum. Due to its high construction efficiency, it has been rapidly popularized, but later on, problems such as mold growth on the ground due to low strength and high ground moisture content appeared, which affected the ground function. Therefore, many areas strictly prohibit the use of foamed gypsum and foamed cement in the floors of residential buildings.
[0003] Since 2017, gypsum-based self-leveling mortar has gradually become popular and is widely used as a backfill leveling layer in dry areas of residential buildings. However, most gypsum-based self-leveling mortars are sandless and have limited thermal conductivity, so they cannot be used in floor heating systems in southern regions. In addition, the cohesive strength of gypsum-based self-leveling mortar is relatively low. When used as a backfill leveling layer for thin ceramic tile floors, it is easy to cause hollowing of ceramic tiles. Summary of the invention
[0004] In response to the above problems, the present application provides a self-compacting gypsum concrete backfill and leveling material and its use. The self-compacting gypsum concrete backfill and leveling material and its construction method provided in the present application are an effective supplement to the technical solution for the backfill and leveling layer of the indoor dry area floor of residential buildings. The self-compacting gypsum concrete backfill and leveling material of the present application increases the elastic modulus and density of the material by introducing a special cementitious material system and a well-matched coarse aggregate and fine aggregate. While taking into account the construction pumpability, the material's body tensile strength is greatly improved. When used as a backfill and leveling layer, the construction efficiency is high, the material system is stable and does not crack, and the body tensile strength is high. It can be used for paving the ground with decorative materials such as flooring, and can also be used for pasting fully paved floors, carpets and other floors.
[0005] In one aspect, the present application provides a self-compacting gypsum concrete backfill leveling material, the raw materials of which include, by weight, 40%-70% of cementitious material, 0-30% of filler, 5%-20% of coarse aggregate, 15%-35% of fine aggregate, 0-5% of alkalinity regulator, 0.05%-0.2% of water reducer, 0.05%-0.15% of defoamer, 0.01%-0.06% of water retention thickener and 0.01%-0.05% of retarder.
[0006] In an embodiment of the present application, the cementitious material includes modified natural or industrial by-product anhydrite; and one or both of α-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum and β-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum;
[0007] Optionally, in the cementitious material system, the weight of the modified natural or industrial by-product anhydrite is 40%-80%, and when the cementitious material includes both α-hemihydrate gypsum and β-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 0%-20%, and the weight of the β-hemihydrate gypsum is 0%-40%; when the cementitious material includes α-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 20%-50%; when the cementitious material includes β-hemihydrate gypsum, the weight of the β-hemihydrate gypsum is 20%-50%.
[0008] In the embodiment of the present application, the filler is one or two of heavy calcium carbonate, fly ash and stone powder.
[0009] In an embodiment of the present application, the coarse aggregate is small stones with a particle size of 3-5 mm, wherein the passing rate of 0.075 μm does not exceed 1%, and the passing rate of 4.75 mm sieve does not exceed 20%.
[0010] In an embodiment of the present application, the fine aggregate is sand with a particle size of 0.15-3 mm, wherein the passing rate of 0.075 μm is not more than 10%, and the passing rate of 1.18 mm is not less than 60%.
[0011] In the embodiment of the present application, the alkalinity regulator is any one of lime lime, silicate cement and mineral powder.
[0012] In an embodiment of the present application, the water reducer is a polycarboxylic acid water reducer.
[0013] In an embodiment of the present application, the defoaming agent is a silicone defoaming agent.
[0014] In an embodiment of the present application, the water-retaining thickener is a cellulose ether;
[0015] Optionally, the viscosity of the cellulose ether is 200-2000 mPa·s;
[0016] Optionally, the cellulose ether is selected from any one or a combination of methyl cellulose ether, hydroxypropyl methyl cellulose ether and hydroxyethyl cellulose ether.
[0017] In an embodiment of the present application, the retarder is a protein retarder.
[0018] On the other hand, the present application provides the use of the self-compacting gypsum concrete backfill and leveling material as described above in the laying of wooden floors, carpets and thin-walled tiles. Optionally, the self-compacting gypsum concrete backfill and leveling material is added with water and stirred, transported to the floor to be backfilled and leveled, poured to the required elevation, and then gently vibrated, defoamed and leveled using a swing bar to obtain a finished construction surface.
[0019] The self-compacting gypsum concrete backfill leveling material and its construction method provided by the present application are an effective supplement to the technical solution of the backfill leveling layer of the indoor dry area of residential buildings. The self-compacting gypsum concrete backfill leveling material of the present application increases the elastic modulus and density of the material by introducing a special cementitious material system and a good combination of coarse aggregate and fine aggregate. On the premise of taking into account the construction pumpability, the material's body tensile strength is greatly improved. When used as a backfill leveling layer, the construction efficiency is high, the material system is stable and does not crack, and the body tensile strength is high. It can be used for laying decorative materials such as floors on the ground, and can also be used for pasting fully paved floors, carpets and other floors.
[0020] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.
[0022] An embodiment of the present application provides a self-compacting gypsum concrete backfill leveling material, wherein the raw materials of the self-compacting gypsum concrete backfill leveling material include, by weight, 40%-70% of a cementitious material, 0-30% of a filler, 5%-20% of a coarse aggregate, 15%-35% of a fine aggregate, 0-5% of an alkalinity regulator, 0.05%-0.2% of a water reducer, 0.05%-0.15% of a defoamer, 0.01%-0.08% of a water-retaining thickener, and 0.01%-0.05% of a retarder.
[0023] In an embodiment of the present application, the cementitious material includes modified natural or industrial by-product anhydrite; and one or both of α-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum and β-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum;
[0024] Optionally, in the cementitious material system, the weight of the modified natural or industrial by-product anhydrite is 40%-80%, and when the cementitious material includes both α-hemihydrate gypsum and β-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 0%-20%, and the weight of the β-hemihydrate gypsum is 0%-40%; when the cementitious material includes α-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 20%-50%; when the cementitious material includes β-hemihydrate gypsum, the weight of the β-hemihydrate gypsum is 20%-50%.
[0025] In an embodiment of the present application, the filler is one or two of heavy calcium carbonate, fly ash and stone powder.
[0026] In an embodiment of the present application, the coarse aggregate is small stones with a particle size of 3-5 mm, and the passing rate of 0.075 μm does not exceed 1%, and the passing rate on 4.75 mm sieve does not exceed 20%.
[0027] In an embodiment of the present application, the fine aggregate is sand with a particle size of 0.15-3 mm, wherein the passing rate of 0.075 μm is no more than 10%, and the passing rate of 1.18 mm is no less than 60%.
[0028] In an embodiment of the present application, the alkalinity regulator is any one of lime lime, silicate cement and mineral powder.
[0029] In an embodiment of the present application, the water reducer is a polycarboxylic acid water reducer.
[0030] In an embodiment of the present application, the defoaming agent is a silicone defoaming agent.
[0031] In an embodiment of the present application, the water-retaining thickener is cellulose ether;
[0032] Optionally, the viscosity of the cellulose ether is 200-800 mPa·s;
[0033] Optionally, the cellulose ether is selected from any one or a combination of methyl cellulose ether, hydroxypropyl methyl cellulose ether and hydroxyethyl cellulose ether.
[0034] In an embodiment of the present application, the retarder is a protein retarder.
[0035] The embodiments of the present application also provide the use of the self-compacting gypsum concrete backfill and leveling material as described above in laying wooden floors, carpets and thin-walled tiles. Optionally, the self-compacting gypsum concrete backfill and leveling material is added with water and stirred, transported to the floor to be backfilled and leveled, poured to the required elevation, and then gently vibrated with a swing bar to defoam and level it, so as to obtain a finished construction surface.
[0036] The sources of the materials used in the examples and comparative examples of this application are as follows:
[0037] Hard gypsum comes from Anhui Jinyang High-tech Materials Co., Ltd.; α-semihydrate gypsum comes from Henan Yongtai Gypsum Co., Ltd. α40 model; β-semihydrate gypsum comes from Hubei Xinyangfeng New Building Materials Technology Co., Ltd.; stone powder, lime calcium and 00.075-3mm sand come from Anhui Beside New Building Materials Technology Co., Ltd.; 3-5mm pebbles come from Beijing Ruichanglong Concrete Co., Ltd.; ordinary Portland cement comes from Chengde Jinyu Cement Co., Ltd.; polycarboxylic acid water reducer is Sika (China) Co., Ltd. 540P high-efficiency water reducer; retarder is Beijing Longhu Technology Co., Ltd. Plaster Retard PE gypsum retarder; low-viscosity cellulose ether is Celanese Shanghai Co., Ltd. E230X; defoamer is Beijing Longhu Technology Co., Ltd. P841; special interface agent is Trinseo 3690 type styrene butadiene emulsion (solid content is 25%).
[0038] Example 1
[0039] The present embodiment provides a self-compacting gypsum concrete backfill leveling material, wherein the raw materials of the self-compacting gypsum concrete backfill leveling material include, by weight, 30% modified anhydrite, 20% β-hemihydrate gypsum, 9% stone powder, 15% 3-5mm pebbles, 23% 0.075-3mm sand, 3% ordinary Portland cement (PO 42.5), 0.14% polycarboxylate water reducer, 0.02% retarder, 0.1% defoamer, and 0.04% cellulose ether.
[0040] The construction method of the self-compacting gypsum concrete backfill leveling material provided in this embodiment is as follows: the raw materials of the self-compacting gypsum concrete backfill leveling material are mixed and packaged in the factory and then transported to the construction site. A multifunctional mixer and a self-leveling pump (with a motor power of 45KW) produced by Hebei Shunde Machinery are used to add water, stir, and pump to the construction floor (15 floors). The amount of water added is 18-20%, and the pumping pressure is 1.2MPa. An average of 4cm is poured on the floor heating base. After 14 days in an environment without direct sunlight, rain protection, and ventilation, the base is sealed with a special interface agent, and then 600*800mm floor tiles are thinly pasted. After 14 days, an on-site pull-out strength test is carried out.
[0041] Example 2
[0042] The present embodiment provides a self-compacting gypsum concrete backfill leveling material, wherein the raw materials of the self-compacting gypsum concrete backfill leveling material include, by weight, 30% modified anhydrite, 12% α-hemihydrate gypsum, 15% stone powder, 10% 3-5 mm pebbles, 33% 0.075-3 mm sand, 3% ordinary Portland cement (PO 42.5), 0.12% polycarboxylate water reducer, 0.015% retarder, 0.1% defoamer, and 0.043% cellulose ether.
[0043] The construction method of the self-compacting gypsum concrete backfill leveling material provided in this embodiment is as follows: the raw materials of the self-compacting gypsum concrete backfill leveling material are mixed and packaged in the factory and then transported to the construction site. A multifunctional mixer and a self-leveling pump (with a motor power of 45KW) produced by Hebei Shunde Machinery are used to add water, stir, and pump to the construction floor (13th floor). The amount of water added is 17-19%, and the pumping pressure is 1.2MPa. An average of 4cm is poured on the floor heating base. After 14 days in an environment without direct sunlight, rain protection, and ventilation, the base is sealed with a special interface agent, and a large plate of 1200*600mm is thinly pasted. After 14 days, an on-site pull-out strength test is carried out.
[0044] Example 3
[0045] The present embodiment provides a self-compacting gypsum concrete backfill leveling material, wherein the raw materials of the self-compacting gypsum concrete backfill leveling material include, by weight, 48% modified anhydrite, 15% α-hemihydrate gypsum, 12% 3-5 mm pebbles, 22% 0.075-3 mm sand, 3% lime, 0.17% polycarboxylate water reducer, 0.01% retarder, 0.08% defoamer, and 0.06% cellulose ether.
[0046] The construction method of the self-compacting gypsum concrete backfill leveling material provided in this embodiment is as follows: the raw materials of the self-compacting gypsum concrete backfill leveling material are mixed and packaged in the factory and then transported to the construction site. A multifunctional mixer and a self-leveling pump (with a motor power of 45KW) produced by Hebei Shunde Machinery are used to add water, stir, and pump to the construction floor (13th floor). The amount of water added is 17-19%, and the pumping pressure is 1.2MPa. An average of 4cm is poured on the floor heating base. After 14 days in an environment without direct sunlight, rain protection, and ventilation, the base is sealed with a special interface agent, and a 600*600mm stone is thinly pasted. After 14 days, an on-site pull-out strength test is carried out.
[0047] Comparative Example 1
[0048] The comparative example provides a concrete backfill leveling material, wherein the raw materials of the leveling material include, by weight, 70% modified anhydrite, 27% β-hemihydrate gypsum, 3% ordinary Portland cement (PO 42.5), 0.18% polycarboxylate water reducer, 0.031% retarder, 0.1% defoamer, and 0.025% cellulose ether.
[0049] The construction method of the concrete backfill leveling material provided in this comparative example is as follows: the raw materials of the concrete backfill leveling material are mixed and packaged in the factory and then transported to the construction site. The raw materials are mixed and packaged in the factory and then transported to the construction site. A multifunctional mixer and a self-leveling pump (with a motor power of 30KW) produced by Hebei Shunde Machinery are used to add water for mixing and pumping to the construction floor (14th floor). The amount of water added is 38-41%, and the pumping pressure is 0.8MPa. An average of 4cm is poured on the floor heating base. After 14 days in an environment without direct sunlight, rain protection, and ventilation, the base is sealed with a special interface agent, and then 600*800mm floor tiles are thinly pasted. After 14 days, an on-site pull-out strength test is carried out.
[0050] Comparative Example 2
[0051] The comparative example provides a concrete backfill leveling material, wherein the raw materials of the leveling material include, by weight, 50% modified anhydrite, 27% β-hemihydrate gypsum, 20% 0.075-3 mm sand, 3% ordinary Portland cement (PO 42.5), 0.17% polycarboxylate water reducer, 0.032% retarder, 0.1% defoamer, and 0.03% cellulose ether.
[0052] The construction method of the concrete backfill leveling material provided in this comparative example is as follows: the raw materials of the concrete backfill leveling material are mixed and packaged in the factory and then transported to the construction site. A multifunctional mixer and a self-leveling pump (with a motor power of 30KW) produced by Hebei Shunde Machinery are used to add water for mixing and pumping to the construction floor (16 floors). The amount of water added is 30-33%, and the pumping pressure is 0.85MPa. An average of 4cm is poured on the floor heating base. After 14 days in an environment without direct sunlight, rain protection, and ventilation, the base is sealed with a special interface agent, and then 1200*600mm floor tiles are thinly pasted. After 14 days, an on-site pull-out strength test is carried out.
[0053]
[0054] As can be seen from Table 1, compared with Comparative Example 1 and Comparative Example 2, the self-compacting gypsum concrete for thin tiles prepared by the concrete backfilling and leveling material of Examples 1-3 of the present application has slightly lower fluidity, but the initial fluidity is not less than 110 mm, which is significantly better than the self-compacting commercial concrete, and the fluidity meets the requirements of backfilling and leveling. In terms of mechanical properties, coarse aggregate can significantly improve the material strength, and the compressive strength and flexural strength are significantly improved compared with Comparative Example 2, among which the improvement space of compressive strength is better than that of flexural strength; the addition of coarse aggregate improves the cohesion and bulk tensile strength of gypsum mortar, and the bulk tensile strength of Examples 1-3 is not less than 1.5MPa, which is equivalent to the bulk tensile strength of cement floor mortar.
[0055] Compared with Comparative Examples 1 and 2, the amount of water added to the materials of Examples 1-3 is smaller. The dry bulk density of Examples 1-3 is close to the bulk density of commercial concrete. Among the two cementitious materials, gypsum and cement, the standard viscosity of gypsum is significantly higher than that of cement. Therefore, the dry bulk density of gypsum products is lower than that of cement products with the same mortar-sand ratio and sand ratio. If we start from the density of the materials, the density of the materials in Examples 1-3 is close to that of cement floor mortar, which is also the main reason for the high bulk tensile strength of the materials in Examples 1-3.
[0056] When using cement-based tile adhesive to thinly lay tiles on the backfill leveling layer, in order to prevent the gypsum-based backfill leveling material and cement-based tile adhesive from generating calcium aluminate when encountering open water, causing the interface layer to crack and then failing to bond in the interface layer and its adjacent areas, it is necessary to apply a special interface agent when the moisture content of the backfill leveling layer is lower than 3% to form a dense organic film. When open water enters the ground, it can effectively block calcium sulfate from migrating from the backfill leveling layer to the tile adhesive, or C3A, C2A and other cement active ingredients from migrating into the backfill leveling layer, thereby preventing the formation of calcium aluminate and ensuring good bonding between the tile adhesive and the tiles, and between the tile adhesive and the backfill layer.
[0057] It can be seen from Comparative Examples 1 and 2 that due to the low tensile strength of the backfill leveling layer, in the pull-out test of the ceramic tile floor system, the failure state occurred in the gypsum leveling layer, and the average pull-out strengths were 0.28 MPa and 0.39 MPa, respectively, which were both low and could not meet the requirements of the floor tile system.
[0058] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.
Claims
1. A self-compacting gypsum concrete backfill leveling material, wherein the raw materials of the self-compacting gypsum concrete backfill leveling material include 40%-70% of cementitious material, 0-30% of filler, 5%-20% of coarse aggregate, 15%-35% of fine aggregate, 0-5% of alkalinity regulator, 0.05%-0.2% of water reducer, 0.05%-0.15% of defoamer, 0.01%-0.06% of water retention thickener and 0.01%-0.05% of retarder by weight.
2. The self-compacting gypsum concrete backfill leveling material according to claim 1, wherein: The cementitious material includes modified natural or industrial by-product anhydrite; and one or both of α-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum and β-hemihydrate gypsum prepared from natural or industrial by-product dihydrate gypsum; Optionally, in the cementitious material system, the weight of the modified natural or industrial by-product anhydrite is 40%-80%, and when the cementitious material includes both α-hemihydrate gypsum and β-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 0%-20%, and the weight of the β-hemihydrate gypsum is 0%-40%; when the cementitious material includes α-hemihydrate gypsum, the weight of the α-hemihydrate gypsum is 20%-50%; when the cementitious material includes β-hemihydrate gypsum, the weight of the β-hemihydrate gypsum is 20%-50%.
3. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1-2, wherein: The filler is one or two of heavy calcium, fly ash and stone powder.
4. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1-2, wherein: The coarse aggregate is small stones with a particle size of 3-5 mm, and the passing rate of 0.075 μm does not exceed 1%, and the passing rate of 4.75 mm sieve does not exceed 20%.
5. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1-2, wherein: The fine aggregate is sand with a particle size of 0.15-3 mm, wherein the passing rate of 0.075 μm does not exceed 10%, and the passing rate of 1.18 mm is not less than 60%.
6. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1-2, wherein: The alkalinity regulator is any one of lime lime, silicate cement and mineral powder.
7. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1-2, wherein: The water reducing agent is a polycarboxylic acid water reducing agent.
8. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1 to 2, wherein the defoamer is an organosilicon defoamer.
9. The self-compacting gypsum concrete backfill leveling material according to any one of claims 1 to 2, wherein the water-retaining thickener is cellulose ether; Optionally, the viscosity of the cellulose ether is 200-2000 mPa·s; Optionally, the cellulose ether is selected from any one or a combination of methyl cellulose ether, hydroxypropyl methyl cellulose ether and hydroxyethyl cellulose ether.
10. The self-compacting gypsum concrete backfilling and leveling material according to any one of claims 1 to 2, wherein the retarder is a protein retarder.
11. Use of the self-compacting gypsum concrete backfilling and leveling material according to any one of claims 1 to 10 in laying wooden floors, carpets and thin-walled tiles, optionally, adding water to the self-compacting gypsum concrete backfilling and leveling material, stirring it, transporting it to the floor to be backfilled and leveled, pouring it to the required elevation, and using a swing bar to gently vibrate, defoam and level it, so as to obtain a finished construction surface.
Citation Information
Patent Citations
Gypsum ground leveling mortar and preparation method thereof
CN113511872A
Construction method of gypsum-based indoor floor self-leveling concrete and construction surface structure of gypsum-based indoor floor self-leveling concrete
CN115126189A
Self-leveling, self-compacting and high-strength gypsum-based indoor floor self-leveling concrete as well as preparation method and application thereof