Low-activity polyaspartic acid ester resin as well as preparation method and application thereof
Low-activity polyaspartate resin is generated through solid-liquid phase separation technology, which solves the problem of poor adhesion caused by excessive activity of polyaspartate resin, achieves improved high strength and corrosion resistance, and is suitable for new applications. Energy battery and engine bottom guard protection.
Patent Information
- Application Number
- CN202410889688.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-08
AI Technical Summary
Existing polyaspartate resins are highly reactive when reacting with isocyanates, resulting in poor adhesion and coating performance, making it difficult to meet high protection requirements such as new energy batteries and engine bottom guards.
By using solid-liquid phase separation technology, isophorone diamine is reacted with carbon dioxide to generate a carbamate-containing structure, which reduces the rate of the subsequent Michael addition reaction, controls the degree of reaction, and forms a low-activity polyaspartate resin.
It significantly reduces the reaction rate of polyurea, improves adhesion and chemical corrosion resistance, and is suitable for surface protection materials for new energy batteries and engine bottom guards. It has high strength and impact resistance.
Smart Images

Figure BDA0004927096810000021 
Figure BDA0004927096810000041 
Figure BDA0004927096810000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyaspartic acid ester resin, in particular to a low-activity polyaspartic acid ester resin and a preparation method and application thereof. Background Art
[0002] Polyaspartic acid ester resin is a new type of resin material developed in recent years. It can react with isocyanate to prepare polyurea. It is positioned as a new type of polyurea material with the characteristics of high performance, high weather resistance, and excellent environmental protection performance. It is widely used in coatings, anti-corrosion floors, adhesives and other fields. After the Michael addition reaction, the amino component is a secondary amine instead of a primary amine, which reduces the reaction rate with isocyanate, and the gel time can be adjusted between a few minutes and tens of minutes. Polyaspartic acid ester polyurea has the advantages of low temperature curing, fast curing speed, high hardness, good toughness, thick coating construction, good coating weather resistance, and good chemical corrosion resistance. It has been more and more widely used at home and abroad. Although compared with traditional polyurea materials, the reaction rate with isocyanate has decreased, but for occasions with high protection requirements such as new energy battery PACK and engine bottom guard plate, the reaction rate is still relatively fast, resulting in problems such as poor adhesion to the substrate and poor coating performance. Therefore, the development of a low-activity polyaspartic acid ester resin has a high application value.
[0003] Reducing the reactivity of polyaspartic acid resin materials has always been a hot topic for scientific researchers. Based on the synthesis process of polyaspartic acid resin, some researchers found that after the Michael addition reaction of dibasic primary amine and maleate, primary amine groups will remain in the system. These primary amine groups react quickly with isocyanate, which leads to the unavoidable fast gelation rate during subsequent spraying. Therefore, researchers add specific components to consume the primary amines, such as isocyanate, in the later stage of synthesis. However, this method has relatively harsh process control and cannot guarantee that the secondary amines will not be consumed before all the primary amines are consumed. In addition, researchers have tried to adjust the formula of the combination material, such as using relatively low-activity isocyanate or adjusting the amount of each component of the formula, but due to factors such as the price, supply and demand of raw materials, the actual production cost remains high.
[0004] In this context, the development of a polyaspartic acid resin with low activity and excellent performance has broad application prospects. Summary of the invention
[0005] To solve the above problems, one of the objects of the present invention is to provide a low-activity polyaspartic acid ester resin. The low-activity polyaspartic acid ester resin prepared by the present invention not only has a long applicability period, but also has the advantages of high strength, impact resistance, chemical corrosion resistance, etc., and can be used as a surface protection material for new energy battery PACK and engine bottom guard plate.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A low-activity polyaspartic acid ester resin, the structure of the resin is as follows:
[0008]
[0009] Among them, R1 is one or more of -CH3, -CH2CH3, -CH2CH2CH3, -CH2CH2CH2CH3, and -CH(CH3)CH2CH3.
[0010] In the process of preparing the low-activity polyaspartic acid ester resin of the present invention, the inventors have found that by using solid-liquid phase separation to control the degree of reaction, and utilizing the structural characteristics of isophorone diamine itself, the amino groups on the ring will preferentially react with carbon dioxide in the air to form salts and precipitate, and cannot contact and react with carbon dioxide, so that the amino groups on the chain can be retained for subsequent Michael addition reaction.
[0011] The activity of the carbamate structure and NCO group of the low-activity polyaspartic acid ester resin is significantly lower than that of secondary amines. It can significantly reduce the reaction rate when spraying polyurea, avoiding poor adhesion due to too fast curing when used by customers. It has the characteristics of high strength, impact resistance, and chemical corrosion resistance after cross-linking, and can be used as a surface protection material for new energy battery PACK and engine bottom guard plate.
[0012] Another object of the present invention is to provide a method for preparing low-activity polyaspartic acid ester resin.
[0013] A method for preparing the above-mentioned low-activity polyaspartic acid ester resin, the method comprising the following steps:
[0014] S1: reacting isophorone diamine with carbon dioxide to precipitate an intermediate containing a carbamate structure;
[0015] S2: The intermediate undergoes Michael addition reaction with maleic acid ester to obtain low-activity polyaspartic acid ester resin.
[0016] In one embodiment of the present invention, the molar ratio of carbon dioxide to isophoronediamine in S1 is greater than 1.
[0017] Exemplarily, the carbon dioxide in S1 can come from readily available air or its source. Preferably, when air is used to provide carbon dioxide, the air flow rate is 10-100 ml / min, preferably 40-60 ml / min. The provision of carbon dioxide is a conventional way to obtain carbon dioxide during organic synthesis. The present invention can also introduce carbon dioxide by other means, and the effect is not significantly different from the introduction of carbon dioxide by air.
[0018] In one embodiment of the present invention, the reaction in S1 is carried out in a solvent; preferably, the solvent is selected from polar solvents, preferably one or more of ethanol, propanol, and n-butanol; preferably, the mass ratio of isophorone diamine to the solvent is 1:2-10, preferably 1:4-6.
[0019] In one embodiment of the present invention, the reaction temperature in S1 is 30-50°C, preferably 40-50°C; the reaction time is 2-6h, preferably 4-6h.
[0020] Exemplarily, isophorone diamine is selected from WANAMINE IPDA, and its reaction mechanism with carbon dioxide in S1 is:
[0021]
[0022] During the preparation of the above-mentioned intermediate containing a carbamate structure, due to the characteristics of the WANAMINE IPDA structure, the carbon dioxide in the air will preferentially form a salt with the primary amine on the ring, and the solid substance will be rapidly precipitated after being generated and cannot come into contact with carbon dioxide, resulting in the retention of the amino group on the chain.
[0023] In one embodiment of the present invention, the maleate in S2 is an ester obtained by reacting maleic acid with a C1-C4 alcohol, preferably one or more of dimethyl maleate, diethyl maleate, dipropyl maleate, dibutyl maleate, and diisobutyl maleate, more preferably dimethyl maleate and / or diethyl maleate.
[0024] In one embodiment of the present invention, the molar amount of maleate in S2 is 1 to 2 times, preferably 1.5 to 2.0 times, the molar amount of the intermediate.
[0025] In one embodiment of the present invention, the reaction in S2 is carried out in a solvent; preferably, the solvent is selected from aprotic solvents, preferably one or more of xylene, dimethyl sulfoxide, and dimethylformamide; preferably, the mass ratio of the intermediate containing a carbamate structure to the solvent is 1:2-8, preferably 1:2-5.
[0026] In one embodiment of the present invention, the reaction temperature in S2 is 40-60°C, preferably 45-55°C; the reaction time is 24-48h, preferably 36-48h.
[0027] Exemplarily, taking diethyl maleate as an example, the reaction mechanism of S2 is:
[0028]
[0029] Another object of the present invention is to provide a use of a low-activity polyaspartic acid ester resin.
[0030] A use of a low-activity polyaspartic acid ester resin, wherein the resin is the polyaspartic acid ester resin described above, or is a polyaspartic acid ester resin prepared by the method described above, and the resin is used in the field of spraying polyurea, preferably for surface protection of composite material new energy battery PACK.
[0031] Another object of the present invention is to provide a spray polyurea.
[0032] A spray polyurea, wherein the polyurea adopts the polyaspartic acid ester resin or the polyaspartic acid ester resin prepared by the method, and the spray polyurea comprises a resin component and a curing agent component.
[0033] In one embodiment of the present invention, the resin component in the spray polyurea comprises the following raw materials in parts by weight: 30-40 parts of polyaspartic acid ester resin, 50-60 parts of low-activity polyaspartic acid ester resin, 0.1-2 parts of dispersant, 0.1-2 parts of anti-settling agent, 5-15 parts of flame retardant, 0.5-2 parts of molecular sieve, 1-4 parts of coupling agent, 0.1-1 parts of defoaming agent, and 0.1-1 parts of leveling agent; preferably, the polyaspartic acid ester resin is a polyaspartic acid ester resin with a diamine structure composed of one or more of alicyclic amine, fatty amine, and aromatic amine, preferably a polyaspartic acid ester resin with an alicyclic amine structure, and more preferably F420 and / or F520.
[0034] In one embodiment of the present invention, the curing agent component in the spray polyurea comprises the following raw materials in parts by weight: 25-75 parts of trimer curing agent and 25-75 parts of prepolymer curing agent; preferably, the trimer curing agent is an HDI trimer, preferably one or more of Asahi Kasei TPA-100, Wanhua HT600, and Wanhua HT300; preferably, the prepolymer curing agent is selected from prepolymers of isocyanate and hydrogen-containing compounds, preferably prepolymers of isocyanate and alcohol compounds, more preferably GB963A-100 and / or GB902-100.
[0035] Another object of the present invention is to provide a method for preparing spray polyurea.
[0036] A method for preparing a spray polyurea, wherein the polyurea adopts the above-mentioned polyaspartic acid ester resin, or the polyaspartic acid ester resin prepared by the above-mentioned method, or is the above-mentioned spray polyurea, and the preparation method comprises the following steps:
[0037] The polyaspartic acid ester resin, the low-activity polyaspartic acid ester resin and the dispersant are mixed, and an anti-settling agent, a flame retardant and a molecular sieve are added to mix to obtain a mixture; a coupling agent, a defoaming agent and a leveling agent are added, mixed and packaged to obtain a resin component; a curing agent is prepared and packaged to obtain a curing agent component.
[0038] Another object of the present invention is to provide a method for using the spray polyurea.
[0039] A method for using a spray polyurea, wherein the polyurea adopts the above-mentioned polyaspartic acid ester resin, or the polyaspartic acid ester resin prepared by the above-mentioned method, or is the above-mentioned spray polyurea, and the method for using the polyurea is as follows: after the resin and the curing agent are preheated, they are sequentially mixed and statically mixed under pressure conditions, and finally sprayed onto the construction surface through atomization, and after drying, the resin component and the curing agent form a polyurea protective layer on the surface; preferably, the method for using the polyurea is preheated to 60-68°C; preferably, the method for using the polyurea is under a pressure condition of 1800-2500PSI.
[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0041] The activity of the carbamate structure and NCO group prepared by the present invention is significantly reduced. When applied to spray polyurea, the drying speed can be increased by 2-3 times to 35-45 minutes, thereby avoiding the problem of poor adhesion due to too fast curing during use by customers, and the problem of delamination and detachment in the later stage.
[0042] In addition, after modification, the carbamate structure exists in the cured product, and the impact resistance and corrosion resistance are also improved compared to traditional polyaspartic acid resins. It can be used as a surface protection material for new energy battery PACKs and engine bottom guard plates, and has broad application prospects. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with specific examples and appended tables, but the implementation method and applicable substrates of the present invention are not limited thereto.
[0044] The raw materials and their sources are shown in Table 1:
[0045] Table 1 Raw materials and sources
[0046] Chemical name factory WANAMINE IPDA Wanhua Chemical Group Co., Ltd. F420 (polyaspartic acid resin) Feiyang Junyan New Materials Co., Ltd. F520 (polyaspartic acid resin) Feiyang Junyan New Materials Co., Ltd. BYK-163(dispersant) BYK Additives (Shanghai) Co., Ltd. BYK-W9010(dispersant) BYK Additives (Shanghai) Co., Ltd. Hydrogenated castor oil (anti-settling agent) Changxing Xiehe Polymer Materials Co., Ltd. Aluminum tripolyphosphate (flame retardant) Changzhou Aked New Material Technology Co., Ltd. Ammonium tripolyphosphate (flame retardant) Guangzhou Yinyuan New Materials Co., Ltd. 800 mesh molecular sieve (molecular sieve) Guangzhou Xinci Environmental Protection Materials Co., Ltd. BYK-4510(coupling agent) BYK Additives (Shanghai) Co., Ltd. BYK-4509 (coupling agent) BYK Additives (Shanghai) Co., Ltd. BYK-085(defoaming agent) BYK Additives (Shanghai) Co., Ltd. BYK-A530(defoaming agent) BYK Additives (Shanghai) Co., Ltd. BYK-3550(leveling agent) BYK Additives (Shanghai) Co., Ltd. GARAMITE-7305(leveling agent) BYK Additives (Shanghai) Co., Ltd. Propanol Maclean Chemical Reagents Ltd. TPA-100 (trimer curing agent) Asahi Kasei HT300 (trimer curing agent) Wanhua Chemical Group Co., Ltd. GB963A-100 (prepolymer curing agent) Feiyang Junyan New Materials Co., Ltd. GB902-100 (prepolymer curing agent) Feiyang Junyan New Materials Co., Ltd. Dimethyl Maleate Shanghai Aladdin Biochemical Technology Co., Ltd. Diethyl Maleate Shanghai Aladdin Biochemical Technology Co., Ltd. Dipropyl Maleate Maclean Chemical Reagents Ltd. Ethanol Maclean Chemical Reagents Ltd. n-Butanol Maclean Chemical Reagents Ltd. Xylene Shanghai Aladdin Biochemical Technology Co., Ltd. Dimethyl sulfoxide Shanghai Aladdin Biochemical Technology Co., Ltd. dimethylformamide Maclean Chemical Reagents Ltd.
[0047] Impact resistance: The resin and curing agent are sprayed on the galvanized steel plate according to the formula to prepare the paint film, and the impact resistance and deformation test are tested according to the national standard GB / T1732 "Determination of impact resistance of paint film".
[0048] Adhesion test: Tested in accordance with the national standard GB / T5210-2006 "Pull-off adhesion test for paints and varnishes".
[0049] Salt spray resistance test: The resin and curing agent are sprayed on the galvanized steel plate according to the formula to prepare a paint film to form a coating film with a film thickness of 50μm. The salt spray resistance of the coating film under 900h is tested with reference to GB-T1771-2007.
[0050] The specific preparation process of the carbamate structure intermediate and the low-activity polyaspartic acid ester resin involved in this scheme is as follows.
[0051] Example 1
[0052] (1) Preparation of intermediates containing carbamate structure:
[0053] The reaction is carried out in a 1L three-necked flask. First, 85g of isophorone diamine and 340g of ethanol are added to the reaction system, and the stirring speed is controlled to be 200r / min; a needle with a diameter of 1.63 mm is inserted into a rubber stopper of a bottleneck, and air with a flow rate of 40ml / min is introduced into the bottom of the three-necked flask to generate bubbles in the solution. Another needle is fixed on the rubber stopper of another neck as a gas outlet; the reaction temperature is controlled to be 30°C, and the transparent solution gradually becomes a milky white turbid liquid, and the bubbling reaction is continued for 2h; after stopping the reaction, a white precipitate will appear. The white precipitate is filtered, washed three times with 30mL of anhydrous ethanol, dried at room temperature in a fume hood for 24 hours, and then dried in a vacuum for another 24 hours, and ground with a mortar to obtain a loose white powder, i.e., the intermediate A1 containing a carbamate structure.
[0054] (2) Preparation of low-activity polyaspartic acid ester resin:
[0055] First, add 232g of xylene into a three-necked flask with mechanical stirring, then add 116g of the obtained amino acid structure intermediate into the solvent, control the stirring speed to 200r / min, and stir for 60min until it is stirred evenly; then, add 144g of dimethyl maleate dropwise into the above system, control the reaction temperature to 40°C, and the reaction time to 24h; after the reaction, perform thin film evaporation at a temperature of 120°C to separate the solvent and excess maleate to obtain low-activity polyaspartic acid ester resin B1.
[0056] Example 2
[0057] (1) Preparation of intermediates containing carbamate structure:
[0058] The reaction is carried out in a 1L three-necked flask. First, 85g of isophorone diamine and 425g of propanol are added to the reaction system, and the stirring speed is controlled to be 250r / min; a needle with a diameter of 1.63 mm is inserted into a rubber stopper of a bottleneck, and air with a flow rate of 50ml / min is introduced into the bottom of the three-necked flask to generate bubbles in the solution. Another needle is fixed on the rubber stopper of another neck as a gas outlet; the reaction temperature is controlled to be 40°C, and the transparent solution gradually becomes a milky white turbid liquid, and the bubbling reaction is continued for 4h; after stopping the reaction, a white precipitate will appear. The white precipitate is filtered, washed three times with 30mL of anhydrous ethanol, dried at room temperature in a fume hood for 24 hours, and then dried in a vacuum for another 24 hours, and ground with a mortar to obtain a loose white powder, i.e., the intermediate A2 containing a carbamate structure.
[0059] (2) Preparation of low-activity polyaspartic acid ester resin:
[0060] First, add 348g of dimethyl sulfoxide into a three-necked flask with mechanical stirring, then add 116g of the obtained amino acid structure intermediate into the solvent, control the stirring speed to 250r / min, and stir for 60min until it is stirred evenly; then slowly add 129g of diethyl maleate dropwise into the above system, control the reaction temperature to 50°C, and the reaction time to 36h; after the reaction, perform thin film evaporation at a temperature of 150°C to separate the solvent and excess maleate to obtain low-activity polyaspartic acid ester resin B2.
[0061] Example 3
[0062] (1) Preparation of intermediates containing carbamate structure:
[0063] The reaction is carried out in a 1L three-necked flask. First, 85g of isophorone diamine and 510g of n-butanol are added to the reaction system, and the stirring speed is controlled to be 200r / min; a needle with a diameter of 1.63 mm is inserted into a rubber stopper of a bottleneck, and air with a flow rate of 60ml / min is introduced into the bottom of the three-necked flask to make the solution produce bubbles. Another needle is fixed on the rubber stopper of another neck as a gas outlet; the reaction temperature is controlled to be 50°C, and the transparent solution gradually becomes a milky white turbid liquid, and the bubbling reaction is continued for 6h; after stopping the reaction, a white precipitate will appear. The white precipitate is filtered, washed three times with 30mL of anhydrous ethanol, dried at room temperature in a fume hood for 24 hours, and then dried in a vacuum for another 24 hours, and ground with a mortar to obtain a loose white powder, i.e., the intermediate A3 containing a carbamate structure.
[0064] (2) Preparation of low-activity polyaspartic acid ester resin:
[0065] First, 464 g of dimethylformamide was added into a three-necked flask with mechanical stirring, and then 116 g of the intermediate containing amino formic acid structure was added into the solvent, the stirring speed was controlled at 200 r / min, and the stirring was carried out for 60 min until the stirring was uniform; then 100 g of dipropyl maleate was slowly added dropwise into the above system, the reaction temperature was controlled at 55 ° C, and the reaction time was 48 h; after the reaction was completed, the solvent and excess maleate were separated by thin film evaporation at a temperature of 130 ° C to obtain low-activity polyaspartic acid ester resin B3.
[0066] Example 4
[0067] (1) Preparation of intermediates containing carbamate structure:
[0068] The reaction is carried out in a 1L three-necked flask. First, 85g of isophorone diamine and 340g of ethanol are added to the reaction system, and the stirring speed is controlled to be 250r / min; a needle with a diameter of 1.63 mm is inserted into a rubber stopper of a bottleneck, and air with a flow rate of 40ml / min is introduced into the bottom of the three-necked flask to generate bubbles in the solution. Another needle is fixed on the rubber stopper of another neck as a gas outlet; the reaction temperature is controlled to be 40°C, and the transparent solution gradually becomes a milky white turbid liquid, and the bubbling reaction is continued for 4h; after stopping the reaction, a white precipitate will appear. The white precipitate is filtered, washed three times with 30mL of anhydrous ethanol, dried at room temperature in a fume hood for 24 hours, and then dried in a vacuum for another 24 hours, and ground with a mortar to obtain a loose white powder, i.e., the intermediate A4 containing a carbamate structure.
[0069] (2) Preparation of low-activity polyaspartic acid ester resin:
[0070] First, add 580g of xylene into a three-necked flask with mechanical stirring, then add 116g of the obtained amino acid structure intermediate into the solvent, control the stirring speed to 250r / min, and stir for 60min until it is stirred evenly; then slowly add 86g of diethyl maleate dropwise into the above system, control the reaction temperature to 60°C, and the reaction time to 36h; after the reaction, perform thin film evaporation at a temperature of 120°C to separate the solvent and excess maleate to obtain low-activity polyaspartic acid ester resin B4.
[0071] The application of the low-activity polyaspartic acid ester resin prepared above in the field of spray polyurea comprises a resin component and a curing agent component.
[0072] The resin and curing agent components are listed in Table 2.
[0073] Comparative Example 1
[0074] Compared with Example 1, the difference is that the polyaspartic acid ester resin F420 is 95 parts and B1 is 0 parts.
[0075] The resin and curing agent components are listed in Table 2.
[0076] Comparative Example 2
[0077] Compared with Example 2, the difference is that the polyaspartic acid ester resin F520 is 95 parts and B2 is 0 parts.
[0078] The resin and curing agent components are listed in Table 2.
[0079] Table 2 Amount of each component of resin and curing agent
[0080] Resin components Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 F420 (polyaspartic acid resin) 35 - 35 - 95 - F520 (polyaspartic acid resin) - 35 - 35 - 95 B1 (patent embodiment 1) 60 - - - - - B2 (Patent Example 2) - 60 - - - - B3 (patent embodiment 3) - - 60 - - - B4 (Patent Example 4) - - - 60 - - BYK-163(dispersant) 0.5 - - 0.1 0.5 - BYK-W9010(dispersant) - 0.1 2 - - 0.1 Hydrogenated castor oil (anti-settling agent) 0.5 0.5 0.1 2 0.5 0.5 Aluminum tripolyphosphate (flame retardant) - 2 - 15 - 2 Ammonium tripolyphosphate (flame retardant) 2 - 5 - 2 - 800 mesh molecular sieve (molecular sieve) 0.5 0.5 0.5 2 0.5 0.5 BYK-4510(coupling agent) 0.5 - 1 - 0.5 - BYK-4509(coupling agent) - 0.5 - 4 - 0.5 BYK-A530(defoaming agent) 0.5 - 0.1 - 0.5 - BYK-085(defoaming agent) - 0.5 - 1 - 0.5 BYK-3550(leveling agent) 0.5 - 0.1 - 0.5 - GARAMITE-7305(leveling agent) - 0.5 - 1 - 0.5 Curing agent component - - - - - - TPA-100 55 55 - - 55 55 HT300 - - 55 55 - - GB963A-100 45 - 45 - 45 - GB902-100 - 45 - 45 - 45
[0081] The resin and curing agent were prepared according to the dosage of Table 2. After weighing the polyaspartic acid ester resin and the low-activity polyaspartic acid ester resin and the dispersant and mixing them evenly, an anti-settling agent was added, and the mixture was dispersed by stirring. Then, a flame retardant and a molecular sieve were added and mixed evenly to obtain a mixture. Finally, a coupling agent, a defoaming agent and a leveling agent were added, mixed evenly and packaged to obtain a resin component. The production humidity was controlled to 10%, and the curing agent was prepared according to the formula and packaged.
[0082] Before spraying, the resin and curing agent are preheated to specific temperature and pressure conditions, and then initially mixed and statically mixed in a mass ratio of 1:0.5. Finally, they are atomized and sprayed onto the surface of the battery PACK. After drying, the resin components and curing agent form a protective layer on the surface.
[0083] The test conditions and results are listed in Table 3.
[0084] Table 3 Performance comparison after spraying
[0085] Example 1 Example 1 Example 1 Example 1 Comparative Example 1 Comparative Example 2 Testing standards Preheating temperature ℃ 60 64 68 60 64 64 - Spraying pressure PSI 1800 2000 2200 2500 2200 2200 - Drying speed / min 35 43 38 44 15 20 Visual inspection Sagging thickness / mm 1.5 1.2 1.8 2.0 3.2 2.7 GB / T9264-2012 Shock Test No damage No damage No damage No damage There are cracks There are cracks GB / T1732 Impact deformation / mm 1.2 1.6 1.5 1.3 1.7 1.8 GB / T1732 Adhesion / MPa 9.5 9.2 9.6 9.8 6.2 5.8 GB / T5210-2006 Salt spray resistance (900h) pass pass pass pass Failed Failed GB / T1771-2007
[0086] As can be seen from the above table, this low-activity polyaspartic acid resin has obvious advantages over polyaspartic acid resins such as F420 and F520. From the data of drying speed and adhesion, it can be seen that the reaction rate is significantly reduced, the drying speed can be increased by 2-3 times to 35-45min, the adhesion to the substrate is significantly improved, and the sag thickness is reduced to less than 2.0mm, which is due to the structure of carbamate and the lower activity of NCO than the secondary amine group. In addition, the cured product has improved impact resistance and corrosion resistance compared with traditional polyaspartic acid resins. The coating has passed the 900h salt spray resistance test and has broad application prospects in the surface protection of new energy battery PACK and engine bottom guard plate.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A low-activity polyaspartic acid ester resin, characterized in that: The structure of the resin is as follows: Wherein, R1 is one or more of -CH3, -CH2CH3, -CH2CH2CH3, -CH2CH2CH2CH3, and -CH(CH3)CH2CH3.
2. A method for preparing the low-activity polyaspartic acid ester resin according to claim 1, characterized in that: The method comprises the following steps: S1: reacting isophorone diamine with carbon dioxide to precipitate an intermediate containing a carbamate structure; S2: The intermediate undergoes Michael addition reaction with maleate to obtain low-activity polyaspartic acid ester resin.
3. The method according to claim 2, characterized in that The molar ratio of carbon dioxide to isophorone diamine in S1 is greater than 1; Preferably, when air is used to provide carbon dioxide, the air flow rate is 10-100 ml / min, preferably 40-60 ml / min; and / or, the reaction in S1 is carried out in a solvent; Preferably, the mass ratio of isophorone diamine to solvent is 1:2-10, preferably 1:4-6; And / or, the reaction temperature in S1 is 30-50° C., preferably 40-50° C.; the reaction time is 2-6 h, preferably 4-6 h.
4. The method according to claim 2, characterized in that The maleate in S2 is an ester obtained by reacting maleic acid with a C1-C4 alcohol, preferably one or more of dimethyl maleate, diethyl maleate, dipropyl maleate, dibutyl maleate, and diisobutyl maleate, more preferably dimethyl maleate and / or diethyl maleate; and / or, the molar amount of the maleate in S2 is 1 to 2 times, preferably 1.5 to 2.0 times, the molar amount of the intermediate; and / or, the reaction in S2 is carried out in a solvent; Preferably, the mass ratio of the carbamate structure-containing intermediate to the solvent is 1:2-8, preferably 1:2-5; And / or, the reaction temperature in S2 is 40-60° C., preferably 45-55° C.; the reaction time is 24-48 h, preferably 36-48 h.
5. A use of a low-activity polyaspartic acid ester resin, wherein the resin is the polyaspartic acid ester resin according to claim 1, or the polyaspartic acid ester resin prepared by the method according to any one of claims 2 to 4, and the resin is used in the field of spraying polyurea, preferably for surface protection of composite material new energy battery packs.
6. A spray polyurea, wherein the polyurea is the polyaspartic acid ester resin according to claim 1 or the polyaspartic acid ester resin prepared by the method according to any one of claims 2 to 4, characterized in that: The spray polyurea comprises a resin component and a curing agent component.
7. The spray polyurea according to claim 6, characterized in that The resin component in the spray polyurea comprises the following raw materials in parts by weight: 30-40 parts of polyaspartic acid ester resin, 50-60 parts of low-activity polyaspartic acid ester resin, 0.1-2 parts of dispersant, 0.1-2 parts of anti-settling agent, 5-15 parts of flame retardant, 0.5-2 parts of molecular sieve, 1-4 parts of coupling agent, 0.1-1 parts of defoaming agent, and 0.1-1 parts of leveling agent; Preferably, the polyaspartic acid ester resin is a polyaspartic acid ester resin having a diamine structure composed of one or more of alicyclic amine, fatty amine, and aromatic amine, preferably a polyaspartic acid ester resin having an alicyclic amine structure, more preferably F420 and / or F520.
8. The spray polyurea according to claim 6, characterized in that The curing agent component in the spray polyurea comprises the following raw materials in parts by weight: 25-75 parts of trimer curing agent and 25-75 parts of prepolymer curing agent; Preferably, the trimer curing agent is an HDI trimer, preferably one or more of Asahi Kasei TPA-100, Wanhua HT600, and Wanhua HT300; Preferably, the prepolymer curing agent is selected from prepolymers of isocyanate and hydrogen-containing compounds, preferably prepolymers of isocyanate and alcohol compounds, more preferably GB963A-100 and / or GB902-100.
9. A method for preparing a spray polyurea, wherein the polyurea is the polyaspartic acid ester resin according to claim 1, or the polyaspartic acid ester resin prepared by the method according to any one of claims 2 to 4, or the spray polyurea according to any one of claims 5 to 8, characterized in that: The preparation method comprises the following steps: Polyaspartic acid ester resin, low-activity polyaspartic acid ester resin and dispersant are mixed, and an anti-settling agent, a flame retardant and a molecular sieve are added to prepare a mixture; a coupling agent, a defoaming agent and a leveling agent are added, mixed and packaged to obtain a resin component; and a curing agent is prepared and packaged to obtain a curing agent component.
10. A method for using a spray polyurea, wherein the polyurea is the polyaspartic acid ester resin according to claim 1, or the polyaspartic acid ester resin prepared by the method according to any one of claims 2 to 4, or the spray polyurea according to any one of claims 5 to 8, characterized in that: The method of use is as follows: after preheating the resin and curing agent, they are sequentially mixed under pressure, statically mixed, and finally sprayed onto the construction surface through atomization. After drying, the resin component and curing agent form a polyurea protective layer on the surface. Preferably, the method of use is preheated to 60-68°C; Preferably, the method of use is under a pressure condition of 1800-2500 PSI.
Citation Information
Patent Citations
Polyaspartic acid ester composition as well as preparation method and application thereof
CN112876956A
Flexible polyurethanes for flexible packaging adhesives without aromatic amine migration
CN116075536A
Preparation method of high-hardness polyaspartic acid ester polyurea
CN117624540A
Method and apparatus for treating bone fractures, and / or for fortifying and / or augmenting bone, including the provision and use of composite implants, and novel composite structures which may be used for medical and non-medical applications
US20200305936A1
GB902-100