Conductive hydrogel as well as preparation method and application thereof
By introducing hydrophobic and hydrophilic functional groups into the hydrogel, and combining the reaction of tertiary ammonia monomers with haloalkanes, a hydrogel with excellent electrical conductivity and mechanical properties was prepared, which solved the problem of poor hydrogel mechanical properties and electrolyte condensation. It solves the problem of weak adhesive properties and achieves high strength and stable conductive properties, making it suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202311652856.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-10-08
AI Technical Summary
Existing hydrogels have poor mechanical properties and are difficult to be directly applied in practice. Electrolyte hydrogels have weak performance due to extremely hydrophilic and mutually repellent electrolytes. In addition, the inorganic small molecule salt conductive medium has the risk of salt loss and is difficult to use for a long time. or save.
Design a conductive hydrogel containing hydrophobic functional groups and hydrophilic functional groups. By regulating the molar ratio of hydrophobic functional groups and hydrophilic functional groups, the swelling of the hydrogel is inhibited, giving it conductive properties and high strength, and through the tertiary ammonia monomer Prepared by solvent exchange after reaction with haloalkanes, a gel with excellent electrical conductivity and mechanical properties is formed.
It achieves the high strength, stability and good conductivity of the conductive hydrogel, which can be used under a variety of conditions and is suitable for flexible sensors and human behavior monitoring. It does not require other salt additives and avoids the conductive performance caused by salt loss. reduce.
Smart Images

Figure CN118745256A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials, and in particular relates to a conductive hydrogel and a preparation method and application thereof. Background Art
[0002] Hydrogel is a gel material with a three-dimensional network structure and water as the medium. It has high similarity and compatibility with biological tissues, and therefore has great potential application value in the fields of wearable devices, artificial skin, biosensors, etc. However, due to the presence of a large amount of water in the hydrogel, its mechanical properties are poor and it is difficult to directly apply it in practice. Electrolyte hydrogel, due to the presence of ionizable groups, has good conductivity and can monitor various physiological activities through changes in electrical signals. It is widely used in biosensors, but there are also problems such as extremely hydrophilic electrolytes and mutual repulsion, resulting in poor performance. At present, there are usually two strategies to optimize the mechanical properties of hydrogels while giving them good conductivity:
[0003] (1) Inhibiting the swelling of the electrolyte hydrogel and improving its mechanical properties by introducing other interactions into the electrolyte hydrogel. For example, introducing trivalent iron ions into polyacrylic acid gel to form a coordination effect with the dissociated carboxylate groups, while introducing polyvinyl alcohol to give it a large number of hydrogen bonds to improve its mechanical properties, or introducing carbon nanotubes into natural sodium alginate hydrogel to enhance its mechanical properties.
[0004] (2) Prepare hydrogel materials with strong mechanical properties in advance, and then introduce conductive media such as inorganic salts to give them conductive properties. For example, lithium chloride is introduced into polyacryloyl glycinamide hydrogels with extremely strong hydrogen bonding to give them conductivity; potassium chloride is introduced into double-layer composite hydrogels, etc.
[0005] However, both of the above strategies rely on post-addition, which involves cumbersome steps. In addition, hydrogel materials using inorganic small molecule salts as conductive media are at risk of salt loss, making them difficult to use or preserve for a long time. Summary of the invention
[0006] In order to overcome the problems existing in the above-mentioned prior art, one of the purposes of the present invention is to provide a conductive hydrogel. The mechanical properties of the hydrogels in the prior art are generally poor. In order to solve the problem of poor mechanical properties, the inventors have proposed a new conductive hydrogel after long-term practice. The conductive hydrogel has both hydrophobic functional groups and hydrophilic functional groups. On the one hand, the hydrophobic ionizable groups are used to inhibit the swelling of the hydrogel while giving the hydrogel material conductive properties and high strength, so that it will not be deformed and damaged when subjected to force in actual application. On the other hand, the presence of the hydrophilic functional group allows the hydrogel to retain a certain amount of water, inhibiting the excessively strong hydrophobic effect to ensure the migration of internal ions.
[0007] A second object of the present invention is to provide a method for preparing a conductive hydrogel.
[0008] A third object of the present invention is to provide a flexible sensor.
[0009] A fourth object of the present invention is to provide a flexible conductive device.
[0010] A fifth object of the present invention is to provide the application of the above-mentioned conductive hydrogel in robots, biomedical prostheses, flexible wearable devices or artificial skin.
[0011] In order to achieve the above object, the technical solution adopted by the present invention is:
[0012] The first aspect of the present invention is to provide a conductive hydrogel, wherein the conductive hydrogel comprises a conductive polymer; the conductive polymer has a structure shown in formula (I),
[0013]
[0014] Wherein, R1 and R2 are each independently selected from H, C 1~3 The alkyl group;
[0015] R3 is selected from amide, hydroxyl, amino, C 1~5 Alkoxycarbonyl, hydroxy substituted C 1~5 Alkoxycarbonyl, amino substituted C 1~5 Alkoxycarbonyl;
[0016] R4 is C 1~6 The alkyl group;
[0017] R5 is C 10~20 The alkyl group;
[0018] M is selected from at least one of O and N.
[0019] Preferably, the C 1~3 The alkyl group is selected from -CH3, -CH2CH3, -CH2CH2CH3, -CH(CH3)2.
[0020] Preferably, the C 1~6 The alkyl group is C 1~6 Branched alkyl or C 1~6 of a straight chain alkyl group.
[0021] Preferably, the C 10~20 The alkyl group is C 10~20 Branched alkyl or C 10~20 of a straight chain alkyl group.
[0022] Preferably, R5 is C 12~18 Preferably, R5 is C 14~18of alkyl.
[0023] Preferably, said R1 and R2 are each independently selected from H, -CH3.
[0024] Preferably, in the conductive polymer, -N + The molar percentage of the (CH3)2R5 functional group is 5-30%; the molar percentage of the R3 functional group is 70-95%; further preferably, in the conductive polymer, -N + The molar percentage of the (CH3)2R5 functional group is 10-25%; the molar percentage of the R3 functional group is 75-90%. If there is too strong a hydrophobic effect in the conductive hydrogel, a larger phase separation region will be generated inside the gel, which is not conducive to the transmission of ions. Therefore, the present invention adjusts the hydrophobic functional group (-N + The molar ratio of (CH3)2R5) and hydrophilic functional group (R3) is adjusted to retain a certain amount of water in the gel while inhibiting hydrophobic interactions to a certain extent.
[0025] Preferably, the conductive polymer is selected from:
[0026]
[0027] The second aspect of the present invention provides a method for preparing the conductive hydrogel provided in the first aspect of the present invention, comprising the following steps:
[0028] S1: polymerizing a tertiary amino monomer and a hydrophilic monomer, and then reacting with a halogenated alkane to obtain an organic gel; or, reacting a tertiary amino monomer with a halogenated alkane, and then polymerizing with a hydrophilic monomer to obtain an organic gel;
[0029] S2: exchanging solvents between the organic gel and water to obtain the conductive hydrogel;
[0030] The halogenated alkane is R5X, where X is F, Cl, Br, or I;
[0031] The hydrophilic monomer is
[0032] The tertiary amino monomer is
[0033] The R1, R2, R3, R4, R5 and M are as defined above.
[0034] Preferably, the molar ratio of the hydrophilic monomer to the tertiary amino monomer is (2-19):1.
[0035] Preferably, the tertiary amino monomer is selected from:
[0036]
[0037] More preferably, the tertiary amino monomer is selected from at least one of dimethylaminoethyl acrylate, dimethylaminopropyl acrylate, dimethylaminoethyl methacrylate, and dimethylaminopropyl methacrylate; and even more preferably, the tertiary amino monomer is selected from dimethylaminoethyl acrylate.
[0038] Preferably, the hydrophilic monomer is selected from at least one of acrylamide, hydroxyethyl acrylate and hydroxyethyl methacrylate; further preferably, the hydrophilic monomer is selected from acrylamide.
[0039] Preferably, the step S1 comprises: mixing a tertiary amino monomer, a hydrophilic monomer, an initiator, a cross-linking agent, and a solvent to undergo a polymerization reaction, and then reacting with a halogenated alkane to obtain an organic gel;
[0040] Alternatively, a tertiary amino monomer is reacted with a halogenated alkane, and then mixed with a hydrophilic monomer, an initiator, a crosslinking agent, and a solvent to undergo a polymerization reaction to obtain an organic gel.
[0041] Further preferably, the step S1 is: under the protection of an inert gas, a tertiary amino monomer, a hydrophilic monomer, an initiator, a crosslinking agent, and a solvent are mixed and subjected to a photocuring polymerization reaction for 6 to 10 hours, and then reacted with a halogenated alkane at 50 to 70° C. for 20 to 30 hours to obtain an organic gel;
[0042] Alternatively, under the protection of an inert gas, the tertiary amino monomer is reacted with a halogenated alkane at 50-70° C. for 20-30 hours, and then mixed with a hydrophilic monomer, an initiator, a crosslinking agent, and a solvent and subjected to a photocuring polymerization reaction for 6-10 hours to obtain an organic gel.
[0043] Preferably, UV irradiation is used in the photocuring polymerization reaction.
[0044] Preferably, the initiator is selected from at least one of α-ketoglutaric acid, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, and (2,4,6-trimethylbenzoyl)diphenylphosphine oxide.
[0045] Preferably, the cross-linking agent is selected from at least one of N,N-methylene acrylamide, 1,4-butanediol diacrylate and polyethylene glycol diacrylate.
[0046] Preferably, the solvent is selected from at least one of methanol, dichloromethane, dimethyl sulfoxide and dimethylformamide; more preferably, the solvent is selected from dimethyl sulfoxide.
[0047] Preferably, the step S2 is: immersing the organogel in water to perform solvent exchange 2 to 5 times to obtain the conductive hydrogel.
[0048] Preferably, X is Cl, Br, or I; more preferably, X is Br or I; and even more preferably, X is Br.
[0049] The third aspect of the present invention provides a flexible sensor, comprising the conductive hydrogel provided by the first aspect of the present invention.
[0050] A fourth aspect of the present invention provides a flexible conductive device, comprising the conductive hydrogel provided by the first aspect of the present invention.
[0051] The fifth aspect of the present invention provides the use of the conductive hydrogel provided in the first aspect of the present invention in a robot, a biomedical prosthesis, a flexible wearable device or an artificial skin.
[0052] The beneficial effects of the present invention are as follows: the conductivity of the conductive hydrogel in the present invention is 0.1-1 S / m, the hydrogel has good stability, can be recycled for a long time, and has the advantages of fast response and high sensitivity when applied to sensors. + The (CH3)2R5 functional group makes the hydrogel have excellent electrical conductivity and enhances its mechanical properties, while the R3 hydrophilic group makes the conductive hydrogel have the necessary water content and can inhibit the hydrophobic effect of the conductive hydrogel. The conductive hydrogel in the present invention has good toughness, can resist large deformation without damage, has good recyclability, and still has good stability when recycled 100 times, and is expected to be applied to various fields such as flexible sensors. The conductive hydrogel in the present invention itself has ionizable quaternary ammonium groups and extremely strong hydrophobic effects, and can achieve good conductivity and high strength without other salt additives, and there is no reduction in conductivity caused by the loss of salt additives, and its anions will not be lost during solvent exchange, and the anions in the hydrogel can be replaced by dialysis.
[0053] In the present invention, by introducing a strongly hydrophobic quaternary ammonium group into the hydrogel, the hydrogel is endowed with excellent mechanical properties, electrical conductivity, good ductility, anti-swelling properties and good recycling performance, and can be used under various conditions. The conductive hydrogel in the present invention has good mechanical properties and can be applied to various human behavior monitoring, such as monitoring of hand movements such as palms and elbows. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a diagram showing the conductivity of the hydrogel of Example 1;
[0055] Figure 2 is a stress-strain diagram of the conductive hydrogel during stretching of Example 2;
[0056] Figure 3 is a stress-strain diagram of the conductive hydrogel during stretching of Example 5;
[0057] Figure 4 is a stress-strain diagram of the conductive hydrogel during stretching of Example 6;
[0058] Figure 5 This is a real-time resistance change diagram when applied to finger joint movement monitoring in Example 2;
[0059] Figure 6 is a graph showing the resistance change of the conductive hydrogel of Example 3 during cyclic stretching;
[0060] Figure 7 is a resistance variation diagram of Example 5 under continuously changing strain;
[0061] Figure 8 This is a resistance change diagram of Example 5 under rapid cyclic strain;
[0062] Fig. 9 is a graph showing the resistance change during cyclic stretching of Example 6;
[0063] Fig.10 for Fig. 9 A partial enlarged view of the middle A;
[0064] Fig.11 for Fig. 9 A partial enlarged view of point B in the middle. DETAILED DESCRIPTION
[0065] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be purchased commercially.
[0066] Example 1
[0067] The structural formula of the conductive hydrogel in this example is:
[0068]
[0069] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0070] (1) 1.43 g of dimethylaminoethyl acrylate and 3.31 g of octadecane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0071] (2) 0.94 g acrylamide, 2.9 mg α-ketoglutaric acid, and 3.1 g N-methylene acrylamide were dissolved in 6 mL of the hydrophobic electrolyte monomer solution, DMSO was added, the volume was fixed to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0072] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(AM-co-DMAEA-Q18 30%) .
[0073] The conductive hydrogel in this example is in a white phase separation state. The conductive hydrogel in this example is connected to a circuit and then connected in series with a light bulb. The conductive hydrogel in this example can realize the conduction of the circuit, thereby making the light bulb glow. The conductive properties of the conductive hydrogel can be seen in Figure 1 After testing, the conductivity of the conductive hydrogel in this example was determined to be 0.3 S / m by electrochemical impedance spectroscopy (EIS).
[0074] Example 2
[0075] The structural formula of the conductive hydrogel in this example is:
[0076]
[0077] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0078] (1) 1.43 g of dimethylaminoethyl acrylate and 3.31 g of octadecane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0079] (2) 1.13 g acrylamide, 2.9 mg α-ketoglutaric acid, and 3.1 g N-methylene acrylamide were dissolved in 4 mL of the hydrophobic electrolyte monomer solution, DMSO was added to make the volume to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0080] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(AM-co-DMAEA-Q18 20% ).
[0081] The mechanical properties of the conductive hydrogel in this example were tested by a universal tensile testing machine. The specific test results are as follows: Figure 2 As shown, it can be seen that the conductive hydrogel in this example has good ductility and mechanical properties.
[0082] Example 3
[0083] The structural formula of the conductive hydrogel in this example is:
[0084]
[0085] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0086] (1) 1.43 g of dimethylaminoethyl acrylate and 2.49 g of dodecane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0087] (2) 0.94 g acrylamide, 2.9 mg α-ketoglutaric acid, and 3.1 g N-methylene acrylamide were dissolved in 6 mL of the hydrophobic electrolyte monomer solution, DMSO was added to make the volume to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0088] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(AM-co-DMAEA-Q12 30% )
[0089] Example 4
[0090] The structural formula of the conductive hydrogel in this example is:
[0091]
[0092] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0093] (1) 0.477 g of dimethylaminopropyl acrylate, 0.94 g of acrylamide, 2.9 mg of α-ketoglutaric acid, and 3.1 g of N-methylene acrylamide were dissolved in water, the volume was fixed to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form a tertiary amine-containing hydrogel.
[0094] (2) Dissolve 10 g of octadecane bromide in DMSO, and adjust the volume to 100 mL using DMSO. Dry the tertiary amine hydrogel prepared in step (1) and soak it in the above solution. Heat to 60° C. and react for 24 h to obtain an organogel.
[0095] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(AM-co-DMAPA-Q18 30% ).
[0096] Example 5
[0097] The structural formula of the conductive hydrogel in this example is:
[0098]
[0099] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0100] (1) 1.56 g of dimethylaminopropyl acrylate and 2.77 g of tetradecane bromide were dissolved in DMSO, the volume was fixed to 10 mL, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0101] (2) 2.964 g of hydroxyethyl methacrylate, 2.9 mg of α-ketoglutaric acid, and 35 mg of polyethylene glycol diacrylate were mixed with 1 mL of the hydrophobic electrolyte monomer solution, DMSO was added to make the volume to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0102] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(HEMA-co-DMAPA-Q14 5% ).
[0103] Example 6
[0104] The structural formula of the conductive hydrogel in this example is:
[0105]
[0106] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0107] (1) 1.56 g of dimethylaminopropyl acrylate and 2.77 g of tetradecane bromide were dissolved in DMSO, the volume was fixed to 10 mL, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0108] (2) 2.08 g of hydroxyethyl methacrylate, 2.9 mg of α-ketoglutaric acid, and 3.1 g of N-methylene acrylamide were dissolved in 2 mL of the hydrophobic electrolyte monomer solution, DMSO was added to make the volume to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0109] (3) The organogel was transferred to deionized water and soaked for 48 h, during which the water was changed three times to obtain the conductive hydrogel in this example, which was recorded as p(HEMA-co-DMAPA-Q14 10% ).
[0110] Comparative Example 1
[0111] The hydrogel in this example was prepared by the following preparation method, and the specific synthesis steps are as follows:
[0112] (1) 14.3 g of dimethylaminoacrylate and 3.31 g of octadecane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0113] (2) 0.94 g of hydrophobic ethyl acrylate, 2.9 mg of α-ketoglutaric acid, and 3.1 g of N-methylene acrylamide were dissolved in 6 mL of the hydrophobic electrolyte monomer solution, DMSO was added, the volume was fixed to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0114] (3) The organogel was transferred to deionized water and soaked for 48 hours, during which the water was changed three times to obtain the hydrogel in this example.
[0115] The gel prepared by using hydrophobic ethyl acrylate in this example shrinks extremely in water, resulting in macroscopic phase separation, and the conductivity drops to 0.07 S / m.
[0116] Comparative Example 2
[0117] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0118] (1) 1.43 g of dimethylaminoethyl acrylate and 3.31 g of octadecane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0119] (2) 0.94 g acrylamide, 2.9 mg α-ketoglutaric acid, and 3.1 g N-methylene acrylamide were dissolved in 8 mL of the hydrophobic electrolyte monomer solution, DMSO was added, the volume was fixed to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0120] (3) The organogel was transferred to deionized water and soaked for 48 hours, during which the water was changed three times to obtain the conductive hydrogel in this example.
[0121] Compared with Example 1, the proportion of hydrophobic electrolyte monomers in this example is increased to 40%. Due to the excessive hydrophobicity, the gel needs to be immersed in water for more than 7 days to reach equilibrium, and the preparation cycle is too long.
[0122] Comparative Example 3
[0123] The conductive hydrogel in this example is prepared by the following preparation method, and the specific synthesis steps are as follows:
[0124] (1) 1.43 g of dimethylaminoethyl acrylate and 3.31 g of octane bromide were dissolved in DMSO, the volume was fixed to 10 mL with DMSO, and then the mixture was transferred to a single-necked flask, nitrogen was introduced for gas exchange, and the mixture was heated to 60° C. for reaction for 24 h to obtain a hydrophobic electrolyte monomer solution.
[0125] (2) 0.94 g acrylamide, 2.9 mg α-ketoglutaric acid, and 3.1 g N-methylene acrylamide were dissolved in 6 mL of the hydrophobic electrolyte monomer solution, DMSO was added, the volume was fixed to 10 mL, and then poured into a transparent mold and irradiated with UV for 8 h to form an organogel.
[0126] (3) The organogel was transferred to deionized water and soaked for 48 hours, during which the water was changed three times to obtain the conductive hydrogel in this example.
[0127] Compared with Example 1, this example uses bromooctane. Due to its weak hydrophobicity, the gel absorbs a large amount of water when immersed in water, and its final water content is as high as 98%. The sol directly breaks during the swelling process and has extremely poor mechanical properties.
[0128] Performance Test:
[0129] (1) Sensing application experiment
[0130] A universal tensile testing machine was used to perform continuous tensile tests on the conductive hydrogels obtained in Example 2, Example 5 and Example 6, respectively, with the maximum tensile strain being 100%. The specific test results are as follows: Figure 2 to Figure 4 As shown, Figure 2 This is the stress-strain diagram of the conductive hydrogel during the stretching process of Example 2. Figure 3 is a stress-strain diagram of the conductive hydrogel during stretching of Example 5; Figure 4 : is the stress-strain diagram of the conductive hydrogel during the stretching process of Example 6. Figure 2 to Figure 4 It can be seen that the conductive hydrogel in the present invention has good ductility and mechanical properties.
[0131] The conductive hydrogel prepared in Example 2 was attached to the finger joints, and the fingers were gradually bent to 30°, 60°, and 90°, while the resistance change of the hydrogel was detected. The specific test results are as follows: Figure 5 As shown by Figure 5 It can be seen that the resistance of the conductive hydrogel in Example 2 changes during the bending of the finger, and when the finger is bent to different degrees, the resistance of the gel also changes differently. The test results show that the conductive hydrogel synthesized in Example 2 of the present invention has conductivity and relatively sensitive deformation responsiveness, and can be used as a flexible sensor.
[0132] The resistance change of the conductive hydrogel in Example 3 during the cyclic stretching process is tested. The specific test results are as follows: Figure 6 As shown by Figure 6 It can be seen that when a 20% strain is cyclically applied to the conductive hydrogel, the resistance change rate of the conductive hydrogel also changes in real time with the strain, and its maximum value is stabilized at about 35%. This test shows that the conductive hydrogel in Example 3 has good deformation responsiveness.
[0133] The conductive hydrogel prepared in Example 5 was subjected to continuous tensile tests using a universal tensile testing machine. The specific test results are as follows: Figure 7 As shown, when the tensile strain increases stepwise from 10% to 50%, the resistance of the conductive hydrogel in Example 5 also shows a synchronous stepwise change. The test results show that the conductive hydrogel synthesized in Example 5 of the present invention has a relatively sensitive strain responsiveness.
[0134] The conductive hydrogel prepared in Example 5 was subjected to continuous and rapid stretching tests using a universal tensile testing machine, with a stretching frequency of 0.4 Hz. The specific test results are as follows: Figure 8 As shown. Figure 8 It can be seen that the resistance of the conductive hydrogel also shows a synchronous rapid change. The test results show that the conductive hydrogel synthesized in Example 5 of the present invention still has good response sensitivity to rapid deformation.
[0135] The conductive hydrogel prepared in Example 6 was subjected to 100 consecutive cyclic stretching tests using a universal tensile testing machine, and the maximum tensile strain was 50%. The specific test results are as follows: Fig. 9 As shown, Fig. 9 The local enlarged picture of point A in the middle is as follows Fig.10 As shown, Fig. 9 The local enlarged picture of point B is as follows Fig.11 As shown by Figures 9 to 11 It can be seen that the resistance change trend of the conductive hydrogel is relatively stable in 100 cycles. The test results show that the conductive hydrogel synthesized in Example 6 of the present invention has good responsiveness to continuous cyclic strain, and the conductive hydrogel in Example 6 has good recyclability.
[0136] It can be seen from the experimental results of the above embodiments and comparative examples that the conductive hydrogel provided by the embodiments of the present invention has good conductivity, anti-swelling performance, ductility and deformation responsiveness, and its anti-swelling performance ensures that it can be used in various humid environments and even water environments, that is, it can maintain a stable state in various humid environments or water, and can be used for human behavior monitoring in various scenarios.
[0137] In summary, the present invention first prepares a hydrophobic electrolyte monomer, then copolymerizes the hydrophobic electrolyte monomer and the hydrophilic monomer to form a gel, and finally obtains a hydrogel through solvent exchange, or first prepares a polymer / hydrogel containing a tertiary amino group, then modifies it with a halogenated alkane, and finally obtains a hydrogel through solvent exchange, wherein the molar ratio of the hydrophobic electrolyte group and the hydrophilic group in the conductive hydrogel is 1: (2.3-19). The preparation method of the present invention is simple in process and mild in reaction conditions. The prepared conductive hydrogel has good conductivity and recyclability, and can be used for various human behavior monitoring in air or humid environments. Therefore, the conductive hydrogel in the present invention can be used in the field of flexible sensors, including soft robots, biomedical prostheses, human flexible electronic devices, artificial skin and other fields, and is particularly suitable for use in scenes where large deformations will occur, such as: human motion monitoring, or suitable for use in humid environments, such as underwater monitoring.
[0138] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A conductive hydrogel, characterized in that: The conductive hydrogel comprises a conductive polymer; the conductive polymer has a structure shown in formula (I), Wherein, R1 and R2 are each independently selected from H, C 1~3 The alkyl group; R3 is selected from amide, hydroxyl, amino, C 1~5 Alkoxycarbonyl, hydroxy substituted C 1~5 Alkoxycarbonyl, amino substituted C 1~5 Alkoxycarbonyl; R4 is C 1~6 The alkyl group; R5 is C 10~20 The alkyl group; M is selected from at least one of O and N.
2. The conductive hydrogel according to claim 1, characterized in that: The R1 and R2 are each independently selected from H, -CH3.
3. The conductive hydrogel according to claim 1, characterized in that: The conductive polymer is selected from:
4. The method for preparing the conductive hydrogel according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: polymerizing a tertiary amino monomer and a hydrophilic monomer, and then reacting with a halogenated alkane to obtain an organic gel; or, reacting a tertiary amino monomer with a halogenated alkane, and then polymerizing with a hydrophilic monomer to obtain an organic gel; S2: exchanging solvents between the organic gel and water to obtain the conductive hydrogel; The halogenated alkane is R5X, where X is F, Cl, Br, or I; The hydrophilic monomer is The tertiary amino monomer is Said R1, R2, R3, R4, R5 and M are as defined in any one of claims 1 to 3.
5. The method for preparing the conductive hydrogel according to claim 4, characterized in that: The molar ratio of the hydrophilic monomer to the tertiary amino monomer is (2-19):
1.
6. The method for preparing the conductive hydrogel according to claim 4, characterized in that: The tertiary amino monomer is selected from:
7. The method for preparing the conductive hydrogel according to claim 4, characterized in that: The step S1 is: mixing a tertiary amino monomer, a hydrophilic monomer, an initiator, a cross-linking agent, and a solvent to undergo a polymerization reaction, and then reacting with a halogenated alkane to obtain an organic gel; Alternatively, a tertiary amino monomer is reacted with a halogenated alkane, and then mixed with a hydrophilic monomer, an initiator, a crosslinking agent, and a solvent to undergo a polymerization reaction to obtain an organic gel.
8. A flexible sensor, characterized in that: The conductive hydrogel comprises the conductive hydrogel according to any one of claims 1 to 3.
9. A flexible conductive device, characterized in that: The conductive hydrogel comprises the conductive hydrogel according to any one of claims 1 to 3.
10. Use of the conductive hydrogel according to any one of claims 1 to 3 in robots, biomedical prostheses, flexible wearable devices or artificial skin.