Low-smoke halogen-free B1-level flame-retardant cable and preparation method thereof
Through the combination of modified magnesium hydroxide, aluminum hypophosphite and modified montmorillonite, the problem of toxic smoke and gas when burning cables is solved, and the low-smoke halogen-free B1 level flame retardant performance and environmental protection are improved. The safety and reliability of the cable are ensured.
Patent Information
- Application Number
- CN202411123076.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cable materials produce a large amount of toxic smoke and gas when burned, making it difficult to meet the B1 flame retardant standard. Adding a large amount of flame retardants leads to a decrease in mechanical properties, affecting service life and environmental pollution.
Modified magnesium hydroxide and aluminum hypophosphite are used as flame retardants, combined with modified montmorillonite as a flame retardant synergist. Through specific coupling treatment and material ratio, the flame retardant performance and environmental protection of the cable are improved. Linear low-density polyethylene, ethylene-vinyl acetate copolymer and ethylene-octene copolymer are grafted with environmentally friendly materials such as maleic anhydride to form a stable network structure to enhance the flame retardant effect.
The preparation of low-smoke halogen-free B1-level flame-retardant cables has been achieved, which improves the cable's flame-retardant performance and environmental protection, reduces smoke release, improves the mechanical properties and service life of the material, and reduces the risk of environmental pollution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, and in particular to a low-smoke halogen-free B1-level flame-retardant cable and a preparation method thereof. Background Art
[0002] With the rapid development of modern science and technology, cables are increasingly used in various industries such as electricity, communications, construction, and transportation. However, frequent cable fire accidents not only cause huge economic losses, but also seriously threaten people's lives. Therefore, the research and development of cable materials with excellent flame retardant properties, especially low-smoke halogen-free B1 flame retardant cables, has become an important research direction in the current cable industry.
[0003] Cable fires have the characteristics of fast spread, fierce fire, and high smoke and toxic gases. Traditional cable materials often produce a large amount of toxic halogen gas and thick smoke when burning, which not only increases the difficulty of fire fighting, but also seriously hinders the evacuation of personnel and even causes casualties. Therefore, the development of low-smoke and halogen-free flame-retardant cable materials is of great significance to improving the safety and reliability of cable use.
[0004] B1 flame-retardant cables refer to cables that can maintain structural integrity for a certain period of time under the action of flames, and produce no or only a small amount of toxic gases and smoke. This type of cable has low smoke, low toxicity, and high flame retardant properties. It can effectively suppress the spread of fire when a fire occurs, and buy precious time for personnel evacuation and fire fighting. B1 flame-retardant cables are widely used in residential, commercial buildings, underground facilities, petrochemical, aerospace, military and other fields, and are crucial to ensure the safe operation of cable lines.
[0005] Although the cable materials currently on the market have flame retardant properties to a certain extent, the following problems still exist: some cables produce a lot of smoke and toxic gases when burning, making it difficult to meet the B1 flame retardant standard, that is, the cable can maintain integrity for a certain period of time under the action of flames without producing a large amount of toxic smoke. In order to improve the flame retardant properties, some cable materials have added a large amount of inorganic flame retardants, resulting in a significant decrease in the mechanical properties and processing properties of the cable, affecting the service life and installation efficiency of the cable. Or harmful substances may be generated during production and use, causing environmental pollution.
[0006] Based on this, the present invention proposes a novel low-smoke halogen-free B1 grade flame retardant cable and a preparation method thereof. Summary of the invention
[0007] The present invention provides a low-smoke halogen-free B1-level flame-retardant cable and a preparation method thereof, which improves the flame retardancy of the cable while also making the cable environmentally friendly.
[0008] The technical solution of the present invention is as follows: In the first aspect, the present invention proposes a low-smoke halogen-free B1 grade flame-retardant cable, wherein the cable sheath is composed of the following raw materials in parts by weight: 50-55 parts of linear low-density polyethylene, 25-35 parts of ethylene-vinyl acetate copolymer, 10-12 parts of ethylene octene copolymer grafted maleic anhydride, 65-75 parts of flame retardant, 16-22 parts of flame retardant synergist, 2-3 parts of antioxidant, and 1-2 parts of lubricant.
[0009] As a further technical solution, the mass grafting rate of maleic anhydride in the ethylene octene copolymer grafted with maleic anhydride is 2.6-3%.
[0010] As a further technical solution, the flame retardant includes modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of (10-12): (2-3).
[0011] The preparation method of the modified magnesium hydroxide is as follows: drying the magnesium hydroxide at 80-90°C for 2-3h, then adding the magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring it into a slurry, slowly adding an aluminate coupling agent, stirring at a speed of 550-650r / min for 40-50min, drying at 55-65°C for 60-80min, and crushing it to obtain the modified magnesium hydroxide.
[0012] As a further technical solution, the usage ratio of the magnesium hydroxide, the ethanol aqueous solution and the aluminate coupling agent is (100-120) g: (1-3) mL: (1-1.2) g.
[0013] As a further technical solution, the flame retardant synergist is modified montmorillonite. The preparation method of the modified montmorillonite is: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 75-85°C for 2-3h, and after the reaction is completed, the modified montmorillonite is obtained by filtering and drying.
[0014] As a further technical solution, the weight ratio of the montmorillonite, anhydrous ethanol and vinyl triethoxysilane is (3-4): (12-14): (1-1.2). As a further technical solution, the antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:(1-2):(2-3).
[0015] As a further technical solution, the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:(2-4).
[0016] In a second aspect, the present invention provides a method for preparing a low-smoke halogen-free B1-level flame-retardant cable, wherein the preparation steps of the cable sheath include: Weigh the raw materials according to the proportion, mix the raw materials and place them in an internal mixer for internal mixing for 30-40 minutes at a mixing temperature of 165-175°C, place the internal mixing product in a screw extruder for extrusion, then place the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 125-135°C, and granulate the product.
[0017] The working principle and beneficial effects of the present invention are: 1. The cable of the present invention uses modified magnesium hydroxide and aluminum hypophosphite as flame retardants. The two can form a stable protective layer during the combustion process, isolate oxygen, and release water vapor and other flame-retardant gases at the same time, effectively inhibiting the spread of flames. The modified magnesium hydroxide improves its dispersibility and compatibility with the substrate through specific coupling treatment and other steps, further enhancing the flame retardant effect. Aluminum hypophosphite can decompose at high temperature to produce phosphoric acid and polymetaphosphoric acid, etc., promote the formation of a carbon layer, and improve flame retardant properties.
[0018] 2. The modified montmorillonite in the present invention acts as a flame retardant synergist. Through its unique layered structure and surface modification, it can produce a synergistic effect with the flame retardant during the combustion process, enhance the stability and density of the carbon layer, and thus further improve the flame retardant properties of the cable.
[0019] 3. The cable sheath of the present invention adopts environmentally friendly materials such as linear low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene octene copolymer grafted with maleic anhydride, etc. These materials will not produce toxic hydrogen halide gas when burned, and the smoke release is low, reducing the harm to the environment and personnel.
[0020] 4. The polar groups (such as carboxyl) in the raw material ethylene-octene copolymer grafted with maleic anhydride of the present invention can chemically react or interact with the polar groups (such as hydroxyl, amino, etc.) in the flame retardant, thereby enhancing the interfacial compatibility between the flame retardant and the substrate. This improvement in compatibility helps the flame retardant to be evenly dispersed in the substrate and improves the flame retardant effect; secondly, the grafted maleic anhydride group acts as a "bridge" to closely connect the flame retardant molecules with the POE substrate to form a stable network structure. This structure not only helps the flame retardant to be effectively dispersed in the cable material, but also prevents the flame retardant from falling off during processing or use, maintaining long-lasting flame retardant properties.
[0021] 5. The addition of ethylene octene copolymer grafted with maleic anhydride in the present invention firstly acts as a compatibilizer to enhance the fusion between materials, especially acts on the dispersion of the flame retardant and the flame retardant synergist in the present invention, which also improves the mechanical properties of the material to a certain extent. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1 In this embodiment, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0024] Example 2 In this embodiment, a low-smoke halogen-free B1 flame-retardant cable is provided, wherein the cable sheath is composed of the following raw materials in parts by weight: 50 parts of linear low-density polyethylene, 25 parts of ethylene-vinyl acetate copolymer, 10 parts of ethylene octene copolymer grafted maleic anhydride, 65 parts of flame retardant, 16 parts of flame retardant synergist, 2 parts of antioxidant, and 1 part of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.6%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 5:1; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 80°C for 2h, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 550r / min for 40min, drying at 55°C for 60min, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 100g:1mL:1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 75°C for 2 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3:12:1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1:2; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:2; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 30 minutes at a mixing temperature of 165°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 125°C, and granulating to obtain the product.
[0025] Example 3 In this embodiment, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 55 parts of linear low-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, 12 parts of ethylene octene copolymer grafted maleic anhydride, 75 parts of flame retardant, 22 parts of flame retardant synergist, 3 parts of antioxidant, and 2 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 3%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 4:1; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 90°C for 3 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 650r / min for 50 minutes, drying at 65°C for 80 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 120g:3mL:1.2g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 85°C for 3 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 4:14:1.2; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:2:3; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:4; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 40 minutes at a mixing temperature of 175°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 135°C, and granulating to obtain the result.
[0026] Example 4 In this embodiment, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 50 parts of linear low-density polyethylene, 35 parts of ethylene-vinyl acetate copolymer, 10 parts of ethylene octene copolymer grafted maleic anhydride, 75 parts of flame retardant, 16 parts of flame retardant synergist, 3 parts of antioxidant, and 1 part of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 3%; The flame retardant comprises magnesium hydroxide and aluminum hypophosphite in a weight ratio of 10:3; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 85°C for 2 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 4:12:1.2; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1:3; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:2; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 40 minutes at a mixing temperature of 165°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 135°C, and granulating to obtain the result.
[0027] Comparative Example 1 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0028] Comparative Example 2 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant is modified magnesium hydroxide; the preparation method of modified magnesium hydroxide is: drying magnesium hydroxide at 85°C for 2.5 hours, then adding it to an ethanol aqueous solution containing 50% by weight of ethanol and stirring it into a slurry, slowly adding aluminate coupling agent DL-411, stirring it at a speed of 600r / min for 45 minutes, drying it at 60°C for 70 minutes, and crushing it to obtain the slurry; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0029] Comparative Example 3 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; Wherein, the flame retardant synergist is montmorillonite; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0030] Comparative Example 4 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0031] Comparative Example 5 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 4%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0032] Comparative Example 6 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0033] Comparative Example 7 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of polypropylene grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in polypropylene grafted maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:1.5:2.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0034] Comparative Example 8 In this comparative example, a low-smoke halogen-free B1 flame-retardant cable is provided, and the cable sheath is composed of the following raw materials in parts by weight: 52 parts of linear low-density polyethylene, 30 parts of ethylene-vinyl acetate copolymer, 11 parts of ethylene octene copolymer grafted maleic anhydride, 70 parts of flame retardant, 19 parts of flame retardant synergist, 2.5 parts of antioxidant, and 1.5 parts of lubricant; Among them, the mass grafting rate of maleic anhydride in ethylene octene copolymer grafted with maleic anhydride is 2.8%; The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of 11:2.5; The preparation method of modified magnesium hydroxide is as follows: drying magnesium hydroxide at 85°C for 2.5 hours, then adding magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding aluminate coupling agent DL-411, stirring at a speed of 600 r / min for 45 minutes, drying at 60°C for 70 minutes, and crushing to obtain the modified magnesium hydroxide; the dosage ratio of magnesium hydroxide, ethanol aqueous solution and aluminate coupling agent is 110g:2mL:1.1g; The flame retardant synergist is modified montmorillonite, and the preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 80°C for 2.5 hours, filtered and dried after the reaction is completed to obtain the modified montmorillonite; the weight ratio of montmorillonite, anhydrous ethanol and vinyl triethoxysilane is 3.5:13:1.1; The antioxidant includes antioxidant DLTP and antioxidant 168 in a weight ratio of 1:1.5; the lubricant includes zinc stearate and polyethylene wax in a weight ratio of 1:3; The preparation method of this low-smoke halogen-free B1 grade flame-retardant cable includes the following steps of preparing the cable sheath: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 35 minutes at a mixing temperature of 170°C, placing the internal mixing product in a screw extruder for extrusion, and then placing the twin-screw product in a single-screw extruder for extrusion at a barrel temperature of 130°C, and granulating to obtain the product.
[0035] Test Example 1: The cable sheath materials prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 were tested as follows: Mechanical properties: The cable sheath material was pressed on a flat vulcanizer at (170-180℃)*10min, with a pressure of 15MPa to obtain a test piece with a thickness of 3mm. The performance of the test piece was tested according to the standard of GB / T32129-2015; Smoke density performance: It is measured according to "GB / T17651.2-2021 Determination of smoke density of electric cables or optical cables burning under specific conditions".
[0036] The test results are shown in Table 1 below: Table 1
[0037] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A low-smoke halogen-free B1 flame-retardant cable, characterized in that: The cable sheath is composed of the following raw materials in parts by weight: 50-55 parts of linear low-density polyethylene, 25-35 parts of ethylene-vinyl acetate copolymer, 10-12 parts of ethylene octene copolymer grafted maleic anhydride, 65-75 parts of flame retardant, 16-22 parts of flame retardant synergist, 2-3 parts of antioxidant and 1-2 parts of lubricant.
2. A low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The mass grafting rate of maleic anhydride in the ethylene octene copolymer grafted with maleic anhydride is 2.6-3%.
3. The low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The flame retardant comprises modified magnesium hydroxide and aluminum hypophosphite in a weight ratio of (10-12): (2-3).
4. The low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The preparation method of the modified magnesium hydroxide comprises: drying the magnesium hydroxide at 80-90° C. for 2-3 hours, then adding the magnesium hydroxide to an ethanol aqueous solution containing 50% by weight of ethanol and stirring to form a slurry, slowly adding an aluminate coupling agent, stirring at a rotation speed of 550-650 r / min for 40-50 minutes, drying at 55-65° C. for 60-80 minutes, and crushing to obtain the modified magnesium hydroxide.
5. The low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The usage ratio of the magnesium hydroxide, the ethanol aqueous solution and the aluminate coupling agent is (100-120) g: (1-3) mL: (1-1.2) g.
6. The low-smoke zero-halogen B1 flame-retardant cable according to claim 1, characterized in that: The flame retardant synergist is modified montmorillonite. The preparation method of the modified montmorillonite is as follows: montmorillonite, anhydrous ethanol and vinyl triethoxysilane are mixed, stirred at 75-85° C. for 2-3 hours, and after the reaction is completed, filtered and dried to obtain the modified montmorillonite.
7. The low-smoke zero-halogen B1 flame-retardant cable according to claim 5, characterized in that: The weight ratio of the montmorillonite, anhydrous ethanol and vinyl triethoxysilane is (3-4): (12-14): (1-1.2).
8. The low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The antioxidants include antioxidant DLTP, antioxidant 168 and antioxidant 619F in a weight ratio of 1:(1-2):(2-3).
9. The low-smoke halogen-free B1 flame-retardant cable according to claim 1, characterized in that: The lubricant comprises zinc stearate and polyethylene wax in a weight ratio of 1:(2-4).
10. A method for preparing a low-smoke halogen-free B1 flame-retardant cable according to any one of claims 1 to 9, characterized in that: The preparation steps of the cable sheath include: weighing raw materials according to a proportion, mixing the raw materials and placing them in an internal mixer for internal mixing for 30-40 minutes, the internal mixing temperature is 165-175° C., placing the internal mixing product in a screw extruder for extrusion, then placing the twin-screw product in a single-screw extruder for extrusion, the barrel temperature is 125-135° C., and granulating to obtain the cable sheath.
Citation Information
Cited By
Flame-retardant B1-level sheath material and application thereof in cable
CN120383793A
A flame-retardant b1 class sheath material and its use in cables
CN120383793B