Preparation process of flexible cable sheath material for industrial automation
A flexible cable sheath material is developed using linear low-density polyethylene and a multi-effect flame retardant, enhancing mechanical strength and flame retardancy while avoiding harmful emissions, thus improving safety and environmental performance.
Patent Information
- Application Number
- CN202411195629.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing cross-linked polyethylene cable sheath materials for industrial automation have low oxygen index, poor flame retardancy, and release harmful gases when burning, posing safety hazards and environmental concerns.
A preparation process involving linear low-density polyethylene, methyl vinyl silicone rubber, a multi-effect flame retardant, antioxidant, and lubricant, combined with electron irradiation, to create a flexible cable sheath material with enhanced mechanical strength, heat resistance, and halogen-free flame retardancy.
The resulting sheath material exhibits excellent flexibility, heat resistance, mechanical strength, and stable flame retardancy, with no harmful gas emissions, addressing safety and environmental issues.
Smart Images

Figure BDA0005016294600000031 
Figure BDA0005016294600000041 
Figure BDA0005016294600000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a preparation process of a flexible cable sheath material for industrial automation. Background Art
[0002] At present, many major equipment in large enterprises use cables for the transmission and distribution of electrical energy. As my country's urbanization process accelerates, the power industry develops rapidly, which further promotes the development of industrial automation equipment. In industrial automation equipment, cables are essential equipment components for the operation of equipment, especially for the demand for flexible cables. Flexible cables are specially designed cables, mainly used in occasions that require frequent movement or bending, such as industrial automation, robots, servo motors and other applications. They usually have high flexibility and bending resistance, and can adapt to dynamic working environments.
[0003] Polyethylene (PE) has good chemical stability, puncture resistance and impact resistance, especially good low temperature resistance, and the brittle temperature can generally reach below -50°C. PE has good processing performance and a wide processing temperature range. Because of its abundant raw material resources, moderate price and superior product comprehensive performance, but the performance of ordinary polyethylene materials is insufficient, cross-linking process is often used to make it into cross-linked polyethylene. Cross-linked polyethylene has excellent flexibility and mechanical strength, and is widely used as a cable sheath material in the cable field. However, cross-linked polyethylene itself has a low oxygen index and poor flame retardant performance. It is easy to burn when encountering open flames, which poses a great safety hazard and needs to be improved.
[0004] Common flame retardants on the market are divided into organic flame retardants and inorganic flame retardants. Inorganic flame retardants have poor compatibility with organic polyethylene matrices, which will affect the mechanical strength of the material. Currently, most organic flame retardants are halogen-containing flame retardants. When these halogen flame retardant materials burn, they release a large amount of smoke and toxic and harmful hydrogen halide gases, which seriously affect and cause losses to people's lives and property. Therefore, people now pay more attention to the development and use of halogen-free flame retardants. Based on the above problems, it is urgent to invent a flexible flame retardant cable sheath material for industrial automation to meet the higher demands in the field of cable material technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a preparation process of a flexible cable sheath material for industrial automation.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A preparation process of a flexible cable sheath material for industrial automation, comprising the following steps:
[0008] Linear low-density polyethylene (LLDPE), methyl vinyl silicone rubber, a cross-linking agent, a multi-effect flame retardant, an antioxidant and a lubricant are put into a twin-screw extruder, melt-blended, and irradiated with an electron accelerator after extrusion to obtain a flexible cable sheath material for industrial automation.
[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 60-80 parts of linear low-density polyethylene, 10-18 parts of methyl vinyl silicone rubber, 5-10 parts of cross-linking agent, 5-15 parts of multi-effect flame retardant, 4-12 parts of antioxidant, and 2-6 parts of lubricant.
[0010] Furthermore, the cross-linking agent is a composite cross-linking agent of triallyl cyanurate and triallyl pentaerythritol, and the mass ratio of the two is 2:3.
[0011] Furthermore, the antioxidant is prepared by compounding a phosphite antioxidant and a phenolic antioxidant in a mass ratio of 1:3.
[0012] Furthermore, the lubricant is one of paraffin and stearamide fatty acid.
[0013] The introduction of methyl vinyl silicone rubber can significantly enhance the heat resistance and flexibility of the sheath material. Methyl vinyl silicone rubber contains double bonds, which can cross-link with the linear low-density polyethylene matrix, making the two more tightly bonded and further improving the performance. The cross-linking agent used is a compound cross-linking agent containing multiple allyl ethers of unsaturated structures, which can significantly increase the cross-linking rate and improve production efficiency. The antioxidant used is a compound of phosphite antioxidants and phenolic antioxidants, which can play a synergistic role and greatly enhance the antioxidant properties of the sheath material. The irradiation method of physical cross-linking has high efficiency, low energy consumption and no pollution compared with chemical cross-linking.
[0014] Furthermore, the multi-effect flame retardant is prepared by the following steps:
[0015] S1. In a three-necked flask equipped with a stirring device, tris(hydroxymethyl)aminomethane hydrochloride, triethylamine and N,N-dimethylformamide (DMF) were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 minutes. Then, phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 90°C and kept for reaction for 7 hours. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed 3-4 times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1; the ratio of tris(hydroxymethyl)aminomethane hydrochloride, triethylamine, N,N-dimethylformamide, and phosphorus oxychloride was 16.1g:15mL:100mL:15.3g;
[0016] Tris(hydroxymethyl)aminomethane hydrochloride reacts with phosphorus oxychloride to obtain intermediate 1; the specific reaction process is as follows:
[0017]
[0018] S2. Add 4,4'-sulfonyl dibenzoic acid and toluene to a three-necked flask equipped with a stirring device, mix, heat to 30°C and stir continuously, introduce nitrogen, add intermediate 1 and dicyclohexylcarbodiimide (DCC, dehydrating agent), mix and stir evenly, heat to 45°C, keep warm and react for 55 minutes. After the reaction is completed, filter, remove the solvent by vacuum distillation, wash with anhydrous ethanol 2-3 times, and vacuum dry to obtain intermediate 2; the ratio of 4,4'-sulfonyl dibenzoic acid, toluene, intermediate 1, and dicyclohexylcarbodiimide is 31.1g:150mL:16.5g:20.6g;
[0019] The carboxyl group on 4,4'-sulfonyl dibenzoic acid and the amino group of intermediate 1 undergo an amidation reaction. Under the action of DCC, the reaction can be carried out under relatively mild conditions. By controlling the molar ratio of the two to be close to 1:1 and a slight excess of 4,4'-sulfonyl dibenzoic acid, only one carboxyl group on 4,4'-sulfonyl dibenzoic acid participates in the reaction to obtain intermediate 2. The specific reaction process is as follows:
[0020]
[0021] S3, at room temperature, under nitrogen protection, 2-vinyl-4,6-diamino-1,3,5-triazine, stearic acid, dicyclohexylcarbodiimide and diethyl ether were mixed and stirred evenly in a three-necked flask equipped with a stirring reflux device, the reaction temperature was controlled to 50°C, refluxed for 3 hours, the reaction was completed, filtered, and part of the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 1:3), and the eluent was removed by rotary evaporation to obtain intermediate 3; the ratio of the amount of 2-vinyl-4,6-diamino-1,3,5-triazine, stearic acid, dicyclohexylcarbodiimide and diethyl ether was 14.7 g:28.5 g:20.6 g:120 mL;
[0022] Under the action of dicyclohexylcarbodiimide, 2-vinyl-4,6-diamino-1,3,5-triazine and stearic acid undergo an amidation reaction, and the intermediate 3 is obtained by controlling the molar ratio of the two to be close to 1:1 and the 2-vinyl-4,6-diamino-1,3,5-triazine to be slightly excessive; the specific reaction process is as follows:
[0023]
[0024] S4. After mixing intermediate 2, intermediate 3, dicyclohexylcarbodiimide and N,N-dimethylformamide in a three-necked flask equipped with a stirring device, the mixture was placed in a water bath at 55°C and heated in a water bath for 8 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), and the eluent was removed by rotary evaporation to obtain a multi-effect flame retardant; the ratio of the amount of intermediate 2, intermediate 3, dicyclohexylcarbodiimide and N,N-dimethylformamide was 45.3 g:40.3 g:20.6 g:200 mL;
[0025] Under the catalysis of dicyclohexylcarbodiimide, intermediate 2 and intermediate 3 undergo amidation reaction to obtain a multi-effect flame retardant; the specific reaction process is as follows:
[0026]
[0027] The multi-effect flame retardant prepared by the present invention is based on diphenyl sulfone, which has good high temperature resistance and thermal oxidation resistance, and can generate SO by thermal desulfurization. 2 , sulfurous acid and water can promote the Fries rearrangement reaction of the matrix, accelerate the carbonization of the matrix, and effectively enhance the flame retardant and smoke suppression properties of the matrix; not only that, the multi-effect flame retardant molecule also contains caged phosphonate, long carbon chain and carbon-carbon double bond structure, among which the caged phosphonate structure is a green and environmentally friendly flame retardant with strong stability. When burned, it will promote the formation of carbon layer, inhibit smoke release, and improve the flame retardant and smoke suppression properties of the matrix; and it can synergize with the N element and S element in the molecule to greatly improve the flame retardant properties of the matrix; in addition, the introduced long carbon chain is a methylene chain segment, which is a flexible chain segment, which can not only improve the flexibility of the matrix, but also be interspersed in the polymer chain of the matrix, and be more tightly connected to the matrix, thereby improving the stability of the multi-effect flame retardant; finally, the introduced carbon-carbon double bond can cross-link with the matrix, which can significantly enhance the migration resistance and exudation resistance of the multi-effect flame retardant, so that the multi-effect flame retardant can perform its performance stably for a long time.
[0028] Beneficial effects of the present invention:
[0029] 1. The sheath material prepared by the present invention uses methyl vinyl silicone rubber and linear low-density polyethylene, and cross-links under irradiation, which gives the sheath material excellent flexibility, heat resistance and mechanical strength;
[0030] 2. The cross-linking agent used is a compound cross-linking agent containing multiple allyl ethers with unsaturated structures, which can significantly increase the cross-linking rate and improve production efficiency;
[0031] 3. The antioxidant used is a compound of phosphite antioxidant and phenolic antioxidant, which can play a synergistic role and give the sheath material excellent antioxidant properties;
[0032] 4. The various groups of the prepared multi-effect flame retardant can work synergistically, significantly enhancing the flame retardancy of the sheath material, and can also improve the flexibility of the sheath material. It is halogen-free and environmentally friendly, and has long-term and stable performance;
[0033] Therefore, the sheath material prepared by the present invention has good flexibility, heat resistance and oxidation resistance, high mechanical strength, stable and efficient flame retardant properties, and is halogen-free and environmentally friendly, and has important application value in the field of cable material technology. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Preparation of multi-effect flame retardant:
[0037] S1. In a three-necked flask equipped with a stirring device, 16.1 g of tris(hydroxymethyl)aminomethane hydrochloride, 15 mL of triethylamine and 100 mL of N,N-dimethylformamide were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 min. Then, 15.3 g of phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 90°C and kept for reaction for 7 h. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed 3-4 times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1.
[0038] S2. Add 31.1 g of 4,4'-sulfonyldibenzoic acid and 150 mL of toluene to a three-necked flask equipped with a stirring device, mix, heat to 30°C and stir continuously, introduce nitrogen, add 16.5 g of intermediate 1 and 20.6 g of dicyclohexylcarbodiimide, mix and stir evenly, heat to 45°C, keep warm and react for 55 minutes. After the reaction is completed, filter, remove the solvent by vacuum distillation, wash with anhydrous ethanol 2-3 times, and vacuum dry to obtain intermediate 2;
[0039] S3, at room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring reflux device, 14.7 g of 2-vinyl-4,6-diamino-1,3,5-triazine, 28.5 g of stearic acid, 20.6 g of dicyclohexylcarbodiimide and 120 mL of ether were mixed and stirred uniformly, the reaction temperature was controlled to 50°C, and the reaction was refluxed for 3 h. After the reaction was completed, the reaction was filtered, and part of the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 1:3), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0040] S4. In a three-necked flask equipped with a stirring device, 45.3 g of intermediate 2, 40.3 g of intermediate 3, 20.6 g of dicyclohexylcarbodiimide and 200 mL of N,N-dimethylformamide were stirred and mixed evenly, and then placed in a 55°C water bath and heated in a water bath for 8 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), and the eluent was removed by rotary evaporation to obtain a multi-effect flame retardant.
[0041] Example 2
[0042] Preparation of multi-effect flame retardant:
[0043] S1. In a three-necked flask equipped with a stirring device, 32.2 g of tris(hydroxymethyl)aminomethane hydrochloride, 30 mL of triethylamine and 200 mL of N,N-dimethylformamide were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 min. Then, 30.6 g of phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 90°C and kept for reaction for 7 h. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed 3 times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1.
[0044] S2. Add 62.2 g of 4,4'-sulfonyldibenzoic acid and 300 mL of toluene to a three-necked flask equipped with a stirring device, mix, heat to 30°C and stir continuously, introduce nitrogen, add 33.0 g of intermediate 1 and 41.2 g of dicyclohexylcarbodiimide, mix and stir evenly, heat to 45°C, keep warm and react for 55 min. After the reaction is completed, filter, remove the solvent by distillation under reduced pressure, wash 3 times with anhydrous ethanol, and vacuum dry to obtain intermediate 2;
[0045] S3, at room temperature, under nitrogen protection, in a three-necked flask equipped with a stirring reflux device, 29.4 g of 2-vinyl-4,6-diamino-1,3,5-triazine, 57.0 g of stearic acid, 41.2 g of dicyclohexylcarbodiimide and 240 mL of ether were mixed and stirred uniformly, the reaction temperature was controlled to 50°C, and the reaction was refluxed for 3 h. After the reaction was completed, the mixture was filtered, and some of the solvent was removed by distillation under reduced pressure. The mixture was then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 1:3), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0046] S4. In a three-necked flask equipped with a stirring device, 90.6 g of intermediate 2, 80.6 g of intermediate 3, 41.2 g of dicyclohexylcarbodiimide and 400 mL of N,N-dimethylformamide were stirred and mixed evenly, and then placed in a 55°C water bath and heated in a water bath for 8 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and then purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate in a volume ratio of 5:1), and the eluent was removed by rotary evaporation to obtain a multi-effect flame retardant.
[0047] Example 3
[0048] 60g of linear low-density polyethylene, 10g of methyl vinyl silicone rubber, 5g of a cross-linking agent (prepared by compounding 2g of triallyl cyanurate and 3g of triallyl pentaerythritol), 5g of the multi-effect flame retardant prepared in Example 1, 4g of an antioxidant (prepared by compounding 1g of antioxidant 168 and 3g of antioxidant 1010) and 2g of paraffin are put into a twin-screw extruder, melt-blended, and irradiated with an electron accelerator after extrusion to obtain a flexible cable sheath material for industrial automation;
[0049] The irradiation was performed using a domestically produced GJ-1.5 high-frequency and high-voltage electron accelerator with an energy of 3 MeV and a current of 22 mA; the irradiation dose rate was 5 kGy / time, and the total irradiation dose was 100 kGy.
[0050] Example 4
[0051] 70g of linear low-density polyethylene, 14g of methyl vinyl silicone rubber, 10g of a cross-linking agent (prepared by compounding 4g of triallyl cyanurate and 6g of triallyl pentaerythritol), 10g of the multi-effect flame retardant prepared in Example 1, 8g of an antioxidant (prepared by compounding 2g of antioxidant 168 and 6g of antioxidant 1010) and 4g of stearamide fatty acid were put into a twin-screw extruder, melt-blended, and irradiated with an electron accelerator after extrusion to obtain a flexible cable sheath material for industrial automation;
[0052] The irradiation was performed using a domestically produced GJ-1.5 high-frequency and high-voltage electron accelerator with an energy of 3 MeV and a current of 22 mA; the irradiation dose rate was 5 kGy / time, and the total irradiation dose was 100 kGy.
[0053] Example 5
[0054] 80g of linear low-density polyethylene, 18g of methyl vinyl silicone rubber, 10g of a cross-linking agent (prepared by compounding 4g of triallyl cyanurate and 6g of triallyl pentaerythritol), 15g of the multi-effect flame retardant prepared in Example 1, 12g of an antioxidant (prepared by compounding 3g of antioxidant 168 and 9g of antioxidant 1010) and 6g of stearamide fatty acid were put into a twin-screw extruder, melt-blended, and irradiated with an electron accelerator after extrusion to obtain a flexible cable sheath material for industrial automation;
[0055] The irradiation was performed using a domestically produced GJ-1.5 high-frequency and high-voltage electron accelerator with an energy of 3 MeV and a current of 22 mA; the irradiation dose rate was 5 kGy / time, and the total irradiation dose was 100 kGy.
[0056] Comparative Example 1
[0057] The multi-effect flame retardant in Example 5 was replaced by a commercially available phosphorus-based flame retardant of equal quality, and the remaining steps were the same as those in Example 5.
[0058] Comparative Example 2
[0059] Commercially available cross-linked polyethylene cable material was used.
[0060] Examples 3-5 and comparative examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:
[0061] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" is used to measure the limiting oxygen index of the sample before and after being placed at room temperature for 180 days;
[0062] The smoke density is measured using the national standard GB / T 8323.2-2008 "Plastic smoke generation Part 2: Single chamber method for determination of smoke density test method";
[0063] The induction time of the sample was determined using the national standard GB / T 19466.6-2009 "Plastic Differential Scanning Calorimetry";
[0064] The notched impact strength and tensile strength of the samples were measured using the national standards GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics" and GB / T 1040-2006 "Determination of Tensile Properties of Plastics". The notched impact strength and tensile strength retention rate of the samples were measured before and after hot air oxidation at 180°C for 72 hours.
[0065] The measured results are shown in the following table:
[0066]
[0067]
[0068] It can be seen from the above table that the sheath material prepared in the embodiment of the present invention has good flexibility, good heat resistance and oxidation resistance, stable and efficient flame retardant properties, and has important application value in the field of cable material technology.
[0069] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0070] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A process for preparing a flexible cable sheath material for industrial automation, characterized in that: The following steps are involved: Linear low-density polyethylene, methyl vinyl silicone rubber, a cross-linking agent, a multi-effect flame retardant, an antioxidant and a lubricant are put into a twin-screw extruder, melt-blended, extruded and irradiated to obtain a flexible cable sheath material for industrial automation.
2. The preparation process of the flexible cable sheath material for industrial automation according to claim 1, characterized in that: The multi-effect flame retardant is prepared by the following steps: S1. Mix tris(hydroxymethyl)aminomethane hydrochloride, triethylamine and N,N-dimethylformamide, place in an ice-water bath at 5°C, stir thoroughly for 30 min, add dropwise 15.3 g of phosphorus oxychloride, and control the temperature not to exceed 20°C during the addition. After the addition is complete, react at 90°C for 7 h. After the reaction is complete, filter under reduced pressure, wash, vacuum dry, and grind to obtain intermediate 1. S2, 4,4'-sulfonyldibenzoic acid and toluene were mixed, heated to 30°C and stirred continuously, nitrogen was introduced, intermediate 1 and dicyclohexylcarbodiimide were added, mixed and stirred evenly, reacted at 45°C for 55 minutes, the reaction was completed, filtered, distilled under reduced pressure, washed, and dried in vacuo to obtain intermediate 2; S3, at room temperature, under nitrogen protection, 2-vinyl-4,6-diamino-1,3,5-triazine, stearic acid, dicyclohexylcarbodiimide and diethyl ether were mixed and stirred evenly, and refluxed at 50°C for 3 hours. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain intermediate 3; S4. Stir and mix intermediate 2, intermediate 3, dicyclohexylcarbodiimide and N,N-dimethylformamide, heat in a water bath at 55° C. for 8 h, and when the reaction is finished, perform vacuum distillation, purify by column chromatography, and rotary evaporate to obtain a multi-effect flame retardant.
3. The preparation process of the flexible cable sheath material for industrial automation according to claim 2, characterized in that: In step S1, the ratio of tris(hydroxymethyl)aminomethane hydrochloride, triethylamine, DMF and phosphorus oxychloride is 16.1 g:15 mL:100 mL:15.3 g.
4. The process for preparing the flexible cable sheath material for industrial automation according to claim 2, characterized in that: In step S2, the ratio of the amount of 4,4'-sulfonyldibenzoic acid, toluene, intermediate 1, and dicyclohexylcarbodiimide is 31.1 g: 150 mL: 16.5 g: 20.6 g.
5. The process for preparing the flexible cable sheath material for industrial automation according to claim 2, characterized in that: In step S3, the ratio of 2-vinyl-4,6-diamino-1,3,5-triazine, stearic acid, dicyclohexylcarbodiimide and diethyl ether is 14.7 g:28.5 g:20.6 g:120 mL.
6. The process for preparing the flexible cable sheath material for industrial automation according to claim 2, characterized in that: In step S4, the ratio of the amount of intermediate 2, intermediate 3, dicyclohexylcarbodiimide and N,N-dimethylformamide is 45.3 g:40.3 g:20.6 g:200 mL.
7. The process for preparing the flexible cable sheath material for industrial automation according to claim 1, characterized in that: The raw materials are calculated in parts by weight as follows: 60-80 parts of linear low-density polyethylene, 10-18 parts of methyl vinyl silicone rubber, 5-10 parts of cross-linking agent, 5-15 parts of multi-effect flame retardant, 4-12 parts of antioxidant, and 2-6 parts of lubricant.
8. The process for preparing the flexible cable sheath material for industrial automation according to claim 1, characterized in that: The cross-linking agent is a composite cross-linking agent of triallyl cyanurate and triallyl pentaerythritol, and the mass ratio of the two is 2:
3.
9. The process for preparing the flexible cable sheath material for industrial automation according to claim 1, characterized in that: The antioxidant is prepared by compounding a phosphite antioxidant and a phenolic antioxidant in a mass ratio of 1:3.
Citation Information
Cited By
Special cable suitable for high-torque robot
CN120833938A
A dedicated cable for high-torque robots
CN120833938B