High-toughness plastic toy
By mixing ABS resin with other resins and materials in specific proportions and injection molding, the problem of insufficient toughness of ABS resin materials is solved, the toughness and aesthetics of toys are improved, and environmentally friendly and efficient production results are achieved.
Patent Information
- Application Number
- CN202411096925.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-08
AI Technical Summary
The ABS resin material of existing plastic toys has insufficient toughness, resulting in toys that are easy to break and have poor aesthetics and playability. In addition, traditional improvement methods have problems of environmental pollution, increased costs, and waste of resources.
By mixing ABS resin with SAN resin, PMMA, EMA, EBA, MAGST and SPEP in specific proportions, and blending and extruding granulation through a twin-screw extruder, the ABS graft powder and The proportion of EMA materials is used to enhance the toughness and processing performance of ABS resin.
It significantly improves the toughness, rigidity and impact strength of ABS resin, improves the mechanical properties and surface properties of toys, reduces manufacturing costs, avoids environmental pollution, and meets the needs of high gloss and environmental protection.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of injection molding technology for children's toys, in particular to a high-toughness plastic toy. Background Art
[0002] As people's living standards continue to improve, children's education is increasingly valued by people. When it comes to the choice of children's toys, more parents prefer children's toys that are scientific and interesting. At present, there are many types and styles of children's toys on the market, including abstract educational toys, toys in various animal shapes, toys in various human shapes, etc. Among them, plastic toys are the mainstream of current children's toys. The injection molding process is the main processing method for plastic toy products. The early injection molding method was mainly used to produce thermoplastic plastic products. With the rapid development of the plastics industry and the continuous expansion of the application range of plastic products, the injection molding method has been promoted and applied to the production of thermosetting plastic products and some composite materials. At present, there are more and more types of plastics that can be injection molded, and most plastics can be injection molded.
[0003] In order to further reduce the complexity of the injection molding process and save the manufacturing cost of plastic toys, the existing plastic toys have a relatively simple structure and function. Most of the structures are fixed, very hard, and easy to be damaged. Some connecting parts are easy to break, and the posture cannot be effectively adjusted. The aesthetics and playability are poor. Based on this, Chinese patent CN216604025U discloses a high-toughness humanoid plastic toy, which includes a fixed base and a driving mechanism. A rotating disk is movably arranged in the fixed base, and a humanoid plastic toy body is fixedly arranged on the upper surface of the rotating disk. The humanoid plastic toy body includes a head, a body, legs and arms. The driving mechanism includes a knob, a first bevel gear, a second bevel gear and a driving shaft. The knob is connected to a transmission rod through a transmission rod. The center of the outer surface of the No. 1 bevel gear is fixedly connected, and the No. 1 bevel gear and the No. 2 bevel gear are meshed with each other, so that the high-toughness humanoid plastic toy can effectively play a lighting role, and can automatically rotate for dynamic display, which is more beautiful.
[0004] However, the plastic toys disclosed in the prior art still have the technical problem of insufficient toughness. Specifically, in the scheme disclosed in the prior art, it is necessary to optimize the assembly structure between the toy parts to improve the coordination of the toy movements; but the current plastic toys are mainly made of acrylonitrile-butadiene-styrene copolymer resin, which is often referred to as ABS resin. As one of the five general synthetic resins, ABS resin is widely used in the injection molding process of plastic toys. Unlike the other four general synthetic resins, ABS is a type of non-crystalline polymer blend obtained by rubber toughened styrene-acrylonitrile copolymer, that is, SAN. Although it has some characteristics of engineering plastics, such as excellent rigidity, heat resistance and impact resistance, it can be used to replace engineering plastics in some occasions. However, the low surface hardness, poor weather resistance, opacity and insufficient toughness of pure ABS limit its use as a high-toughness toy substrate. In addition, with the demand trend of thin-walled, lightweight and beautiful toy shell materials, the market has higher and higher requirements for the comprehensive performance of toy materials, and plastic toys with excellent surface properties such as high gloss are obviously more popular with consumers. Traditional high-gloss toy products are mostly achieved through polishing and spraying after plastic molding. These secondary processes have problems such as environmental pollution, increased costs, waste of resources and harm to workers' health, which violates the concept of environmental protection, high efficiency and energy saving. Therefore, the development of resin alloy materials with excellent comprehensive performance and outstanding surface gloss performance has become a hot spot in the research and development of special toy materials. Summary of the invention
[0005] Based on this, it is necessary to provide a high-toughness plastic toy in order to solve the technical problem of how to enhance the material toughness of ABS resin used in children's toys.
[0006] A high-toughness plastic toy is made of ABS resin mixture pellets through injection molding. The ABS resin mixture pellets are composed of 14-22 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 0-10 parts of EMA, 1 part of EBA, 0.13-0.17 parts of MAGST and 1 part of SPEP in parts by mass.
[0007] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0008] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0009] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0010] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 16 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0011] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.16 parts of MAGST and 1 part of SPEP.
[0012] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.17 parts of MAGST and 1 part of SPEP.
[0013] Furthermore, the ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.13 parts of MAGST and 1 part of SPEP.
[0014] In summary, the present invention provides a high-toughness plastic toy, which is made of ABS resin mixture pellets by injection molding. The ABS resin mixture includes, by mass, 14-22 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 0-10 parts of EMA, 1 part of EBA, 0.13-0.17 parts of MAGST and 1 part of SPEP. The high-toughness toy can be made by fully mixing the ABS resin mixture, and then blending and extruding it at 190 to 210° C. through a twin-screw extruder to obtain ABS resin mixture pellets. The ABS resin mixture pellets are dried and then injection molded by an injection molding machine at 200° C. using a preset injection mold. By adjusting different proportions of ABS grafted powder and EMA material, the ABS resin material can be toughened and improved. Therefore, the present invention provides a high-toughness plastic toy that solves the technical problem of how to enhance the material toughness of ABS resin used in children's toys. DETAILED DESCRIPTION
[0015] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation mode of the present invention is described in detail below in conjunction with embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0016] Specifically, ABS resin is a polybutadiene, i.e., a "sea-island" two-phase structure in which PB rubber particles are dispersed in a continuous phase of SAN resin. The PB rubber particles give ABS resin toughness and low-temperature impact resistance, while the SAN resin gives ABS resin rigidity, glossiness and chemical stability. This shows that the toughness, rigidity or impact strength of the resin can be improved by adjusting the content of ABS grafted powder or its components in the resin. Therefore, the preparation of high-toughness ABS resin requires two aspects: one is to adjust the rubber content in the resin; the other is to optimize the processing aid system to improve the processing performance and appearance of the product.
[0017] Specifically, polymethyl methacrylate, or PMMA, is an atactic polymer obtained by free radical polymerization of methyl methacrylate monomers. It has the characteristics of high surface hardness, good heat resistance and excellent gloss performance, and is one of the most transparent plastics currently. However, it also has some relatively serious defects such as poor fluidity, low impact strength and room temperature creep, and it is difficult to meet the toughness requirements of commonly used toy molded products; ABS and PMMA can complement each other in terms of performance when blended. While improving the impact toughness of PMMA, the mechanical properties, surface characteristics and flame retardancy of ABS have been improved to varying degrees.
[0018] Specifically, ethylene-methyl acrylate copolymer, or EMA, is a resin material with excellent mechanical properties, good environmental stress cracking resistance and excellent electrical properties. Through different molding processes, it can be made into products such as films, hoses and profiles, toys and foam sheets. EMA resin is often used in polymer modification and can be used as a compatibilizer and toughening agent for polymers such as ABS, PA, PC, PBT, PET or PP, especially as a compatibilizer and toughening agent for alloys such as PBT / PC or PC / ABS.
[0019] Furthermore, the present invention provides a high-toughness plastic toy, which is formed by injection molding ABS resin mixture pellets, wherein the ABS resin mixture includes: ABS grafted powder, SAN resin, PMMA, EMA, EBA, MAGST and SPEP.
[0020] Among them, SAN resin is the abbreviation of styrene acrylonitrile copolymer resin; EBA is the abbreviation of N-ethylene bis stearamide; MAGST is the abbreviation of magnesium stearate; SPEP is the abbreviation of antioxidant 618.
[0021] The present invention discloses an injection molding method for a high-toughness plastic toy, which comprises the following steps: ABS grafted powder, SAN resin, PMMA, EMA, EBA, MAGST and SPEP in different proportions are fully mixed, and then co-mixed and extruded at 190 to 210° C. by a twin-screw extruder to obtain ABS resin mixture pellets. The ABS resin mixture pellets are dried and then injection molded by an injection molding machine at 200° C. using a preset injection mold. In subsequent experimental steps, the product samples need to be placed in an environment with a temperature of 23° C. and a humidity of 55% for 24 hours before their performance can be tested.
[0022] Specifically, the tensile performance test of the sample is carried out at room temperature in accordance with GB / T 1040.2-2006 standard, with a test speed of 5mm / min. For each test, the number of samples is not less than 5, until a relatively stable and concentrated performance parameter value is obtained; then, the average value is taken as the test value of the performance. The cantilever beam impact test is carried out at room temperature in accordance with GB / T 1843-2008 standard. According to the impact energy range of different samples, a suitable energy hammer is selected for the test. Bending strength: According to ASTMD790, the test span is 60mm, and the load is applied at a speed of 15 / mmmin. Melt flow rate: According to ASTM D1238 standard, the test temperature is 220℃, and the weight is 10KG. Hardness: According to ASTM D785 test, using R scale. Gloss: According to ASTMD785 test.
[0023] In one embodiment, the components of the basic raw materials are fixed as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP, by weight; and the components of EMA are preset to be 0 to 10 parts and divided into five embodiments with a difference of 2. EMA in different proportions is mixed with the above-mentioned basic raw materials and then extruded into granules and injection molded into standard specimens, and the effects of its content on the tensile strength, cantilever beam impact strength and fracture productivity of ABS alloy are revealed as shown in Table 1.
[0024] Table 1: Data on the effect of EMA component content on the mechanical strength of ABS alloy
[0025] From the data in Table 1, it can be seen that with the increase of EMA content, the tensile strength of the alloy shows a decreasing pattern. When the EMA content exceeds 4wt%, the tensile strength decreases rapidly. In addition, impact strength and elongation at break are the two most important indicators for measuring the toughening effect of rubber particles during modification. The effect of EMA content on the cantilever beam impact strength and elongation at break of the alloy is shown in the data in Table 1. Continuing to refer to Table 1, it can be seen that when the EMA content in the alloy increases from 0 to 8wt%, the cantilever beam impact strength increases from 44.9KJ / m 2 Increased to 73.8KJ / m 2 , the elongation at break increased from 11.5% to 28.8%, an increase of 67% and 150% respectively, and the increase was obvious. Moreover, even when the content of EMA was low, the toughening effect was very significant. It can be seen that the good compatibility of EMA with mixtures such as ABS significantly affects the mechanical properties of the alloy. The addition of EMA reduces the interfacial tension between ABS, SAN and PMMA, and improves the compatibility of the three, which can be regarded as a single phase, thereby causing the decrease in the tensile strength of the alloy. With the increase of EMA content, EMA becomes a weak phase. When the content exceeds 4wt%, the tensile strength of the alloy shows a significant downward trend. That is to say, it can be explained that EMA plays a good toughening role in the alloy, which is reflected in the significant improvement of the cantilever beam impact strength and elongation at break of the alloy. On the one hand, the improvement of interfacial compatibility improves the toughness of the alloy; on the other hand, the vinyl contained in EMA also plays a very important role in the toughening effect of the alloy, which can effectively absorb the external energy when the material is subjected to impact. EMA particles are evenly dispersed in the alloy and act as stress concentration points when subjected to stress. These particles can absorb a large amount of energy when subjected to stress and deformation, and at the same time can induce matrix yielding and silver streaks, avoiding brittle failure of the material. The combined effect of these effects significantly improves the toughness of the alloy.
[0026] Further, in another embodiment, the components of the basic raw materials are fixed as follows: 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP, by weight. The ABS grafted powder is mixed with the above-mentioned basic raw materials in a ratio of 14, 16, 18, 20, and 22%, and then extruded into granules and injection molded into standard specimens to reveal the influence of different ratios of ABS grafted powder on the properties of the final ABS resin. The results are shown in Table 2 below.
[0027] Table 2: Effect of different graft powder contents on the mechanical strength of ABS alloy
[0028] The comparative example in Table 2 is the comparative test data of conventional untoughened ABS resin materials available on the market. It can be seen from Table 2 that as the content of ABS grafted powder increases, the tensile strength of ABS resin gradually decreases. When the content of grafted powder in ABS resin is 20%, the performance parameters are equivalent to those of the comparative example. Therefore, when the content of ABS grafted powder is less than 20%, the mechanical properties are better than those of conventional ABS resin materials.
[0029] Thus, the present invention is a high-toughness toy, and several different specific embodiments are further disclosed below: An embodiment of a high-toughness plastic toy is formed by injection molding of ABS resin mixture pellets, wherein the ABS resin mixture comprises, by mass, 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0030] Furthermore, another embodiment of a high-toughness plastic toy is formed by injection molding of ABS resin mixture pellets, wherein the ABS resin mixture comprises, by mass, 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0031] Furthermore, another embodiment of a high-toughness plastic toy is formed by injection molding of ABS resin mixture pellets, wherein the ABS resin mixture comprises, by mass, 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0032] Furthermore, another embodiment of a high-toughness plastic toy is formed by injection molding of ABS resin mixture pellets, wherein the ABS resin mixture comprises, by mass, 16 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
[0033] Furthermore, MAGST, magnesium stearate, can diffuse the surface of the ABS resin product with the surface of the mold metal during injection, and thus can act as a mold release agent to improve the surface gloss of the product, thereby obtaining a plastic toy product with good surface aesthetics. However, MAGST will affect the flow rate of the ABS resin melt in the injection mold, that is, the amount of MAGST needs to meet the preset ratio requirements.
[0034] Specifically, another embodiment of a high-toughness plastic toy is formed by injection molding of ABS resin mixture pellets, wherein the ABS resin mixture, by mass, includes: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.13-0.17 parts of MAGST and 1 part of SPEP. Among them, MAGST can be 0.13, 0.14, 0.15, 0.16 and 0.17 parts respectively. The impact strength test of this embodiment is shown in Table 3.
[0035] Table 3: Data on the influence of different MAGST contents on the material properties of ABS alloy
[0036] Specifically, Comparative Example 1 in Table 3 is the comparative test data of the conventional untoughened ABS resin material on the market. Based on the data in Table 3, it can be seen that: as the amount of MAGST increases, the melt flow rate of ABS resin increases; and after the amount of MAGST is 0.15%, the increase becomes larger; while the impact strength of ABS resin reaches the maximum value when the amount of MAGST is 0.16%, and then decreases. This is because MAGST plays the role of internal lubrication and external lubrication in ABS resin: a part of it is dissolved in ABS resin to play the role of internal lubrication, improve the uniform dispersion of various components of the resin, and when the amount reaches a certain value, the dispersion is best, so the impact strength has a peak; the other part of the undissolved MAGST plays the role of external lubrication. During injection molding, this part of MAGST diffuses to the ABS resin and the metal surface of the mold, which can play the role of a release agent, and then play the role of improving the surface gloss of the plastic product.
[0037] In summary, the present invention provides a high-toughness plastic toy, which is made of ABS resin mixture pellets by injection molding. The ABS resin mixture includes, by mass, 14-22 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 0-10 parts of EMA, 1 part of EBA, 0.13-0.17 parts of MAGST and 1 part of SPEP. The high-toughness toy can be made by fully mixing the ABS resin mixture, and then blending and extruding it at 190 to 210° C. through a twin-screw extruder to obtain ABS resin mixture pellets. The ABS resin mixture pellets are dried and then injection molded by an injection molding machine at 200° C. using a preset injection mold. By adjusting different proportions of ABS grafted powder and EMA material, the ABS resin material can be toughened and improved. Therefore, the present invention provides a high-toughness plastic toy that solves the technical problem of how to enhance the material toughness of ABS resin used in children's toys.
[0038] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0039] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A high-toughness plastic toy, It is characterized in that The ABS resin mixture is made by injection molding. The ABS resin mixture comprises 14-22 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 0-10 parts of EMA, 1 part of EBA, 0.13-0.17 parts of MAGST and 1 part of SPEP in parts by mass.
2. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
3. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 4 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
4. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 14 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
5. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 16 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.15 parts of MAGST and 1 part of SPEP.
6. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.16 parts of MAGST and 1 part of SPEP.
7. A high-toughness plastic toy according to claim 1, Features: The ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.17 parts of MAGST and 1 part of SPEP.
8. A high-toughness plastic toy according to claim 7, Features: The ABS resin mixture particles are calculated by weight as follows: 20 parts of ABS grafted powder, 60 parts of SAN resin, 20 parts of PMMA, 6 parts of EMA, 1 part of EBA, 0.13 parts of MAGST and 1 part of SPEP.
Citation Information
Patent Citations
High-toughness human-shaped plastic toy
CN216604025U
Cited By
A low-bubble plastic toy manufacturing process
CN122939038A