Polylactic acid composite material and preparation method thereof
By using zinc oxide modified plant fiber in polylactic acid materials, the problem of poor antibacterial performance of polylactic acid materials is solved, the antibacterial performance and mechanical properties are improved, and the service life is extended.
Patent Information
- Application Number
- CN202410905266.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-08
AI Technical Summary
Adding plant fibers to polylactic acid materials has poor antibacterial properties and is susceptible to mold, rotting fungi and insects, affecting its use value.
Zinc oxide modified plant fiber is used. Through alkali treatment, colloidal solution infiltration and moist heat treatment technology, zinc oxide particles are coated on the surface of the plant fiber. Combined with polylactic acid compound, the zinc oxide modified plant fiber is formed to improve the antibacterial performance and toughness. .
Significantly improves the antibacterial properties and mechanical properties of polylactic acid composite materials, enhances its resistance to bacteria, mold, and rotting fungi, and extends its service life.
Smart Images

Figure BDA0004932184520000151 
Figure BDA0004932184520000191 
Figure BDA0004932184520000201
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of polymer materials, and in particular relates to a polylactic acid composite material and a preparation method thereof. Background Art
[0002] Polylactic acid (PLA) is a biodegradable material that is widely accepted by the market due to its good biodegradability and biocompatibility and environmental friendliness. PLA is one of the ideal candidate materials to replace petroleum-based plastics, with the characteristics of high transparency, high processability, low toxicity and environmental protection. PLA can be a good choice of packaging material, and can also be used as a food-grade material, and can be used in products that come into direct contact with food, such as straws and cups.
[0003] The use of polylactic acid materials to replace petroleum-based plastics can alleviate the serious white pollution caused by the large-scale use of petroleum-based polymers to the environment, but polylactic acid materials also have certain limitations. For example, the inherent brittleness and single function of polylactic acid limit its scope of application. By adding plant fibers to polylactic acid materials, such as fibers of plants such as balsa wood, bamboo, and sisal, the strength and toughness of polylactic acid materials can be improved. Balsa wood, bamboo, sisal, etc. are plants with a faster growth rate, with low cost and excellent strength, and the fibers of these plants are degradable plant fibers. By adding plant fibers to polylactic acid materials, not only can the mechanical properties of polylactic acid materials be improved, but also because plant fibers are degradable, the polylactic acid material with added plant fibers can still have good degradable properties.
[0004] Although adding plant fibers to polylactic acid materials can improve the mechanical properties of polylactic acid materials and make polylactic acid materials have good biodegradability, polylactic acid materials will inevitably undergo chemical migration. At the same time, polylactic acid materials are often used in food packaging and other fields that are in direct contact with food and prone to bacterial growth. Bacterial growth may affect human health and food quality and safety. Therefore, it is very important to improve the antibacterial ability of polylactic acid materials. In addition, due to the poor corrosion resistance of plant fibers, they are easily attacked by mold, decay fungi and insects, resulting in poor antibacterial properties of polylactic acid materials containing plant fibers, which reduces the use value of polylactic acid materials. Summary of the invention
[0005] The purpose of the present application is to provide a polylactic acid composite material and a preparation method thereof, so as to solve the technical problem that the polylactic acid material containing plant fibers in the prior art has poor antibacterial properties.
[0006] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0007] In a first aspect, the present invention provides a polylactic acid composite material. The polylactic acid composite material of the present invention comprises the following components in parts by weight:
[0008] 40-60 parts of polylactic acid;
[0009] 10-20 parts of zinc oxide modified plant fiber;
[0010] 0-30 parts of copolymer of butylene adipate and butylene terephthalate;
[0011] Polybutylene succinate 0-20 parts.
[0012] The zinc oxide modified plant fiber comprises plant fiber and a zinc oxide coating layer, and the zinc oxide coating layer is coated on the surface of the plant fiber.
[0013] The polylactic acid composite material of the embodiment of the present application is compounded with polylactic acid and zinc oxide modified plant fiber in a specific ratio, and further combined with a copolymer of butylene adipate and butylene terephthalate, polybutylene succinate and other components, so that the polylactic acid composite material has good toughness and degradability, and effectively improves the antibacterial property of the polylactic acid composite material. The polylactic acid composite material of the embodiment of the present application has good degradability, antibacterial property and mechanical property, high tensile strength and high elongation at break.
[0014] In a second aspect, the present invention provides a method for preparing a polylactic acid composite material. The method for preparing a polylactic acid composite material in the present invention is the method for preparing a polylactic acid composite material described above, and comprises the following steps:
[0015] The raw materials including polylactic acid and zinc oxide modified plant fiber are mixed to obtain a polylactic acid mixture;
[0016] The polylactic acid mixture is smelted to obtain a polylactic acid composite material.
[0017] The method for preparing the polylactic acid composite material of the embodiment of the present application performs a smelting treatment on the polylactic acid mixture, so that the components such as polylactic acid in the polylactic acid mixture are melted to form a uniform melt, and the components in the raw materials are fully mixed to obtain a uniform and stable polylactic acid composite material. The polylactic acid composite material prepared by the preparation method of the embodiment of the present application has good toughness, good degradability, and good antibacterial properties, and the zinc oxide particles in the polylactic acid composite material have good dispersibility, and are stably combined with substrates such as polylactic acid, and are not easy to aggregate and precipitate. In addition, the process conditions of the method for preparing the polylactic acid composite material of the embodiment of the present application are well controllable, and the prepared polylactic acid composite material has stable performance and is suitable for industrial large-scale production and application. DETAILED DESCRIPTION
[0018] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0019] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0020] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.
[0021] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0022] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0023] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass in the embodiment description of the present application can be μg, mg, g, kg and other mass units known in the chemical industry.
[0024] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0025] In order to solve the technical problem in the prior art that polylactic acid materials containing plant fibers have poor antibacterial properties, the present application proposes the following technical solution.
[0026] In a first aspect, the present invention provides a polylactic acid composite material. The polylactic acid composite material of the present invention comprises the following components in parts by weight:
[0027] 40-60 parts of polylactic acid;
[0028] 10-20 parts of zinc oxide modified plant fiber;
[0029] 0-30 parts of copolymer of butylene adipate and butylene terephthalate;
[0030] Polybutylene succinate 0-20 parts.
[0031] The zinc oxide modified plant fiber comprises plant fiber and a zinc oxide coating layer, and the zinc oxide coating layer is coated on the surface of the plant fiber.
[0032] The polylactic acid composite material of the present application is effectively improved by adding zinc oxide modified plant fiber in the composite material based on polylactic acid (polylactic acid, PLA), so that the polylactic acid composite material of the present application has good antibacterial properties, and effectively alleviates the infringement of bacteria, mold, rot fungi and insects suffered by the polylactic acid composite material of the present application. At the same time, by coating the zinc oxide coating layer on the surface of the plant fiber, and then compounding the zinc oxide modified plant fiber with PLA, the dispersibility of zinc oxide in the polylactic acid composite material can be effectively improved, the dispersion uniformity of zinc oxide is improved, and the problems such as the aggregation of zinc oxide particles caused by directly adding zinc oxide in PLA are avoided. In addition, the polylactic acid composite material of the present application is effectively improved in a specific range by controlling the ratio of polylactic acid and zinc oxide modified plant fiber, and the tensile strength and elongation at break of the polylactic acid composite material are improved.
[0033] In some embodiments, the weight proportion of zinc oxide modified plant fiber contained in the polylactic acid composite material of the present application embodiment can also be 10 to 15 parts, which can be selected as 10 to 13 parts, 13 to 18 parts, 15 to 20 parts, and 17 to 20 parts. In the exemplary embodiment, the weight proportion of zinc oxide modified plant fiber can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts and other typical but non-limiting proportions, or any proportion between any two numerical ranges. Controlling the weight proportion of zinc oxide modified plant fiber within this range, compounding components such as polylactic acid, effectively improves the toughness and antibacterial ability of the polylactic acid composite material of the present application embodiment.
[0034] In some embodiments, the plant fiber in the zinc oxide modified plant fiber may include at least one of bamboo fiber, balsa fiber, and sisal fiber. These plant fibers have good biodegradability and good toughness. The zinc oxide modified plant fiber prepared from these plant fibers is compounded with polylactic acid, etc., which can not only effectively improve the toughness of the polylactic acid composite material, but also make the polylactic acid composite material have good degradability.
[0035] In some embodiments, the plant fiber in the zinc oxide modified plant fiber is an alkali-treated plant fiber. By alkali-treating the plant fiber, the compatibility of the plant fiber with the polylactic acid material is effectively improved, thereby improving the tensile strength and other mechanical properties of the polylactic acid composite material.
[0036] In some embodiments, the zinc oxide coating layer may include zinc oxide particles. In further embodiments, the particle size D50 of the zinc oxide particles may be 100-300 nm, optionally 100-200 nm, 100-250 nm, 200-300 nm. In an exemplary embodiment, the particle size of the zinc oxide particles may be 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, etc., which are typical but non-limiting particle sizes, or any particle size between any two numerical ranges. The particle size of the zinc oxide particles is controlled within this range, so that the zinc oxide particles are nano zinc oxide particles. On the one hand, the binding force between the zinc oxide particles and the plant fibers is improved, and the structural stability of the zinc oxide-modified plant fibers is improved; on the other hand, the zinc oxide-modified plant fibers are compounded with components such as polylactic acid, thereby further improving the antibacterial properties of the polylactic acid composite material of the embodiment of the present application.
[0037] In some embodiments, the coverage of the zinc oxide coating on the surface of the plant fiber can be 60% to 80%, optionally 60% to 75%, 60% to 70%, 70% to 80%. In an exemplary embodiment, the coverage of the zinc oxide coating on the surface of the plant fiber can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, etc., which are typical but non-limiting sizes, or any size between any two numerical ranges. By controlling the coverage rate of the zinc oxide coating layer on the surface of the plant fiber within this range, the antibacterial properties of the polylactic acid composite material can be effectively improved, while further improving the compatibility of the zinc oxide-modified plant fiber with components such as PLA, improving the brittleness of the polylactic acid-based material, promoting the improvement of the toughness of the polylactic acid composite material, and further improving the mechanical properties of the polylactic acid composite material such as tensile strength and elongation at break.
[0038] In some embodiments, the thickness of the zinc oxide coating layer can be 0.5-1 μm, and can be 0.5-0.8 μm, 0.5-0.7 μm, 0.6-0.9 μm, 0.7-1 μm. In the exemplary embodiment, the thickness of the zinc oxide coating layer can be 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.8 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1 μm, etc., which are typical but non-limiting thicknesses, or any thickness between any two numerical ranges. Controlling the thickness of the zinc oxide coating layer within this range further improves the adhesion of the zinc oxide coating layer on the surface of the plant fiber, improves the structural stability of the zinc oxide modified plant fiber, thereby further improving the stability of the polylactic acid composite material, and promoting the uniform dispersion of zinc oxide in the polylactic acid composite material.
[0039] In some embodiments, the zinc oxide coating layer may include a single-layer structure or a multi-layer structure. In a further embodiment, the number of layers in the zinc oxide coating layer may be 1-7 layers, and may be 3-7 layers. In the exemplary embodiment, the number of layers of the zinc oxide coating layer may be any one of 1 layer, 2 layers, 3 layers, 4 layers, 5 layers, 6 layers, and 7 layers. By controlling the zinc oxide coating layer to be a multi-layer structure, the coverage of the zinc oxide coating layer on the surface of the plant fiber can be increased. By controlling the number of layers of the zinc oxide coating layer within this range, the adhesion of the zinc oxide coating layer on the surface of the plant fiber can be further increased, and the structural stability of the zinc oxide modified plant fiber can be increased. In the exemplary embodiment, the thickness of different layered structures in the zinc oxide coating layer may be the same or different, and is not specifically limited.
[0040] In some embodiments, the zinc oxide modified plant fiber can be prepared by a modification method comprising the following steps:
[0041] Step G10: using the first alkali solution to perform alkali treatment on the plant fiber to obtain alkali-treated plant fiber;
[0042] Step G20: placing the alkali-treated plant fiber in a colloidal solution containing zinc hydroxide particles for infiltration treatment to obtain pretreated plant fiber;
[0043] Step G30: Mix the pretreated plant fiber with the precursor solution and perform wet heat treatment to obtain zinc oxide modified plant fiber.
[0044] There are a large number of micropores and grooves on the surface of plant fibers. After the plant fibers are treated with alkali and then immersed in a colloidal solution, the zinc hydroxide particles contained in the colloidal solution are adsorbed on the surface of the plant fibers, as well as in the surface micropores and grooves. In the subsequent wet heat treatment process, the zinc hydroxide adsorbed in the plant fibers forms zinc oxide under the action of high temperature. At the same time, the zinc hydroxide in the precursor solution is continuously hydrolyzed to form zinc oxide seeds, which grow on the surface of the plant fibers to form zinc oxide nanoparticles.
[0045] Step G10:
[0046] The plant fiber is treated with alkali using the first alkali solution in step G10 to remove impurities in the plant fiber and reduce the hydroxyl content on the surface of the plant fiber. Since the plant fiber has water absorption, it is easy to cause the polylactic acid composite material to degrade in advance, and the compatibility of the plant fiber and polylactic acid is not good, thereby affecting the performance of the polylactic acid material with the plant fiber. The hydroxyl content on the surface of the plant fiber is effectively reduced by alkali treatment, thereby reducing the hydroxyl content on the surface of the zinc oxide modified plant fiber obtained later, reducing the hydrophilicity of the zinc oxide modified plant fiber, improving the compatibility of the zinc oxide modified plant fiber with components such as polylactic acid, and inhibiting the early degradation of the polylactic acid composite material.
[0047] In some embodiments, the first alkali solution may include at least one of a sodium hydroxide solution and a sodium silicate solution. The concentration of the first alkali solution may be 2-7wt%, optionally 2-5wt%, 3-5wt%. In the exemplary embodiment, the concentration of the first alkali solution may be 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, etc., which are typical but non-limiting concentrations, or any concentration between any two numerical ranges.
[0048] In some embodiments, the weight ratio of the plant fiber to the first alkali solution can be 1: (10-20), and can be optionally 1: (10-15). In the exemplary embodiment, the weight ratio of the plant fiber to the first alkali solution can be 1: 10, 1: 11, 1: 12, 1: 13, 1: 14, 1: 15, 1: 16, 1: 17, 1: 18, 1: 19, 1: 20, and other typical but non-limiting weight ratios. The plant fiber is subjected to alkaline alkali treatment with the first alkali solution of these types and concentration ranges, and the weight ratio of the plant fiber to the first alkali solution is controlled within this range, so as to effectively remove impurities in the plant fiber, reduce the hydroxyl content on the surface of the plant fiber, and improve the compatibility of the plant fiber with components such as polylactic acid.
[0049] In some embodiments, the alkali treatment time can be 6 to 24 hours, and can be 10 to 14 hours. In the exemplary embodiment, the alkali treatment time can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, etc., which are typical but non-limiting times, or any time within any two numerical ranges. The alkali treatment time is controlled within this range to further remove impurities in the plant fiber, reduce the hydroxyl content on the surface of the plant fiber, and maintain the toughness of the plant fiber.
[0050] In some embodiments, a dispersant is also added during the alkali treatment process, and the dispersant may include at least one of diaminetetraacetic acid and sodium bisulfite. In a further embodiment, the amount of the dispersant may be 0.5-2wt% of the plant fiber, and may be 0.5-1wt%. In the exemplary embodiment, the amount of the dispersant may be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt% of the plant fiber, etc., which are typical but non-limiting sizes, or any size between any two numerical ranges. By adding a dispersant during the alkali treatment process, and at the same time keeping the amount of the dispersant within this range, the dispersion state of the plant fiber during the alkali treatment process is effectively improved, thereby promoting the plant fiber to fully and evenly contact with the first alkali solution, and effectively improving the alkali treatment effect.
[0051] In some embodiments, after the first alkali treatment, the plant fiber is taken out, and the plant fiber can also be washed and dried to facilitate subsequent processing using the alkali-treated plant fiber. In a further embodiment, water can be used to wash the alkali-treated plant fiber until the washing liquid is neutral. In the exemplary embodiment, the alkali-treated plant fiber can be dried in an 80°C drying oven for 48 hours, and the washed plant fiber can also be dried under reduced pressure. The water content of the alkali-treated plant fiber after drying can be 5 to 8wt%, and can be optionally 5 to 7wt%. In the exemplary embodiment, the water content of the alkali-treated plant fiber after drying can be typical but non-restrictive sizes such as 5wt%, 6wt%, 7wt%, 8wt%, or any size between any two numerical ranges.
[0052] Step G20:
[0053] In step G20, the alkali-treated plant fiber is wetted in the colloidal solution, so that the zinc hydroxide particles in the colloidal solution are adsorbed on the surface of the alkali-treated plant fiber and in structures such as the microporous structure and the groove structure on the surface, and then dried to obtain the pretreated plant fiber. The zinc hydroxide particles in the colloidal solution form abundant hydrogen bonds with the hydroxyl groups on the surface of the alkali-treated plant fiber, so that the zinc hydroxide particles form a strong interaction with the surface of the alkali-treated plant fiber, which helps the zinc hydroxide particles to stably adhere to the surface of the alkali-treated plant fiber and in structures such as the microporous structure and the groove structure.
[0054] In some embodiments, the colloidal solution can be prepared by mixing a first zinc salt solution and an organic base reagent and then subjecting the mixture to a first stirring treatment.
[0055] In some embodiments, the first zinc salt solution may include a solution of a soluble zinc salt such as zinc acetate dihydrate, zinc chloride, zinc sulfate, zinc nitrate, etc. The solvent in the first zinc salt solution may include an organic solvent, such as methanol, ethanol, etc., or may include water, which is not specifically limited, as long as it has good solubility for the soluble zinc salt. In an exemplary embodiment, the first zinc salt solution may be a methanol solution of zinc acetate dihydrate, and the concentration of the methanol solution of zinc acetate dihydrate may be 5wt% to 10wt%. In an exemplary embodiment, it may be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, etc., which are typical or non-limiting values, or any value between any two numerical ranges.
[0056] In some embodiments, the organic alkali reagent may include an organic alkali reagent containing a hydroxyl group. In the exemplary embodiment, the organic alkali reagent may include at least one of monoethanolamine, diethanolamine, triethanolamine, triethylamine, and ethylenediamine. These alkali reagents have good compatibility with the solvent in the first zinc salt solution, and these first alkali reagents also have suitable alkalinity.
[0057] In some embodiments, the organic alkali reagent can be dissolved in a solvent to form an organic alkali reagent solution, and then mixed with the first zinc salt solution. In a further embodiment, the solvent for dissolving the organic alkali reagent can include at least one of water and an organic solvent, and the organic solvent can be an organic solvent miscible with water, such as methanol, ethanol, etc. The solvents for dissolving the organic alkali reagent have good compatibility with the alkali reagent and the solvent in the aforementioned first zinc salt solution.
[0058] In some embodiments, the concentration of the organic base reagent solution can be 0.02-0.04 mol / L. In exemplary embodiments, the concentration of the organic base reagent can be 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, or any other typical or non-limiting values, or any value between any two numerical ranges.
[0059] In some embodiments, the volume ratio of the first zinc salt solution to the organic alkali reagent solution can be (1:0.8) to (1:1.2). In an exemplary embodiment, the first zinc salt solution and the organic alkali reagent solution can be mixed in a volume ratio of 1:1. By controlling the concentration of the organic alkali reagent within this range, and controlling the volume ratio of the first zinc salt solution to the organic alkali reagent within this range, the particle size and concentration of the zinc hydroxide particles in the colloidal solution are further controlled, and the alkali-treated plant fibers are promoted to uniformly adsorb the zinc hydroxide particles, and the uniformity of the zinc oxide coating layer in the subsequently prepared zinc oxide-modified plant fibers is further improved.
[0060] In some embodiments, the temperature of the first stirring treatment can be 50-60°C. In the exemplary embodiment, the temperature of the first stirring treatment can be a typical but non-limiting temperature such as 50°C, 53°C, 55°C, 58°C, 60°C, or any temperature between any two numerical ranges. In a further embodiment, the rotation speed of the first stirring treatment can be 100-500r / min, optionally 100-200r / min. In the exemplary embodiment, the rotation speed of the stirring treatment can be a typical but non-limiting size such as 100r / min, 200r / min, 300r / min, 400r / min, 500r / min, or any size between any two numerical ranges. The temperature and rotation speed of the first stirring treatment are controlled within this range, combined with the first zinc salt solution and the organic alkali reagent, to further control the size of the zinc hydroxide particles in the colloidal solution, promote the uniform adsorption of the zinc hydroxide particles on the surface of the alkali-treated plant fiber, and obtain the pretreated plant fiber with uniform adsorption of zinc hydroxide particles on the fiber surface.
[0061] In some embodiments, the time for the alkali-treated plant fiber to be soaked in the colloidal solution can be 0.5 to 3 minutes, and can be 0.5 to 1 minute. In the exemplary embodiment, the soaking time can be 0.5 minutes, 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, and other typical but non-limiting times, or any time between any two numerical ranges. Controlling the soaking time within this range further promotes the uniform attachment of zinc hydroxide particles to the surface of the alkali-treated plant fiber.
[0062] After the soaking treatment, the taken-out pretreated plant fibers can be dried. In an exemplary embodiment, the drying temperature of the pretreated plant fibers can be 80° C. for 1 hour. The drying treatment promotes the drying of the pretreated plant fibers and helps the pretreated plant fibers maintain good toughness and other mechanical properties.
[0063] Step G30:
[0064] Through step G30, the pretreated plant fiber is mixed with a precursor solution containing zinc hydroxide, subjected to a wet heat treatment at a high temperature, and then dried to obtain zinc oxide-modified plant fiber.
[0065] In some embodiments, the precursor solution can be prepared by mixing a second zinc salt solution and a second alkali solution. The second zinc salt solution can include an aqueous solution of a soluble zinc salt, and the soluble zinc salt can include zinc acetate, zinc chloride, zinc sulfate, zinc nitrate, etc., which are not specifically limited. The second alkali solution can be an aqueous solution containing hydroxide ions, for example, the second alkali solution can include sodium hydroxide, potassium hydroxide, etc., which are not specifically limited.
[0066] In a further embodiment, the concentration of the second zinc salt solution can be 5-10wt%, and can be 5-8wt% optionally. In the exemplary embodiment, the concentration of the second zinc salt can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% and other typical but non-limiting sizes, or any size between any two numerical ranges. The concentration of the second alkali solution can be 2-5wt%, and can be 2-3wt%. In the exemplary embodiment, the concentration of the second alkali solution can be 2wt%, 3wt%, 3wt%, 4wt%, 5wt% and other typical but non-limiting sizes, or any size between any two numerical ranges. The volume ratio of the second zinc salt solution mixed with the second alkali solution can be 1: (20-30), and can be 1: (20-25). In the exemplary embodiment, the volume ratio of the second zinc salt solution mixed with the second alkali solution can be 1: 20, 1: 25, 1: 30 and other typical but non-limiting sizes, or any size between any two numerical ranges. The concentrations of the second zinc salt solution and the second alkali solution are controlled within the range, and the volume ratio of the second zinc salt solution and the second alkali solution is controlled within the range, which effectively promotes the formation of zinc hydroxide in the precursor solution, and at the same time controls the pH value in the precursor solution, further promoting the formation of zinc oxide nanoparticles during the wet heat treatment process.
[0067] In some embodiments, the temperature of the wet heat treatment can be 130-150°C, optionally 130-140°C, 135-150°C. In the exemplary embodiment, the temperature of the wet heat treatment can be 130°C, 131°C, 132°C, 133°C, 134°C, 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, etc., typical but non-limiting temperatures, or any temperature between any two numerical ranges. In the exemplary embodiment, the wet heat treatment can be carried out in an autoclave lined with polytetrafluoroethylene, and the pressure of the wet heat treatment can be set by those skilled in the art according to actual needs. The time of the wet heat treatment can be 0.5-2h, optionally 0.5-1h, 1-2h. In the exemplary embodiment, the time of the wet heat treatment can be a typical but non-restrictive time such as 0.5h, 1h, 1.5h, 2h, or any time between any two numerical ranges. Through the wet heat treatment, the zinc hydroxide particles attached to the surface of the pretreated plant fiber decompose to form zinc oxide particles and water, while the zinc hydroxide in the precursor solution is continuously hydrolyzed to form zinc oxide seeds, and grows on the surface of the fiber to form zinc oxide nanoparticles, so that the zinc oxide nanoparticles are coated on the surface of the plant fiber. During the wet heat treatment process, the zinc oxide nanoparticles interact with the hydroxyl groups on the surface of the plant fiber to form rich hydrogen bonds, thereby facilitating the deposition and stable binding of the zinc oxide nanoparticles on the plant fiber matrix. Subsequently, due to the effect of electrostatic adsorption, the newly added zinc oxide nanoparticles are adsorbed on the nanoparticles previously attached to the surface of the plant fiber, and the newly added zinc oxide nanoparticles are combined with the attached zinc oxide nanoparticles. By controlling the temperature and time of the wet heat treatment within this range, combined with the precursor solution, the loading of zinc oxide nanoparticles on the surface of the plant fibers can be effectively promoted, and the particle size and coverage rate of the zinc oxide nanoparticles can be effectively controlled, thereby further improving the antibacterial properties of the polylactic acid composite material.
[0068] In some embodiments, multiple wet heat treatments may be performed to form a multi-layer structure of zinc oxide coating layers on the surface of the plant fiber.
[0069] In some embodiments, after the pretreated plant fiber is subjected to the wet heat treatment, the fiber is taken out and the fiber can also be washed. In an exemplary embodiment, the fiber obtained by the wet heat treatment can be ultrasonicated with water for 30 minutes. In a further embodiment, the washed zinc oxide modified plant fiber can also be dried. In an exemplary embodiment, the washed zinc oxide modified plant fiber can be vacuum dried at 50° C. for 48 hours.
[0070] The zinc oxide-modified plant fiber prepared by alkali treatment, colloidal solution infiltration treatment and wet heat treatment in the embodiment of the present application has good interfacial compatibility with high molecular polymers such as polylactic acid. At the same time, the zinc oxide-modified plant fiber is compounded with components such as polylactic acid to prepare a polylactic acid composite material, which effectively improves the antibacterial ability of the polylactic acid composite material and makes the polylactic acid composite material have good degradability.
[0071] In some embodiments, the weight fraction of PLA contained in the polylactic acid composite material of the present application embodiment can also be 40-50 parts, 50-60 parts. In the exemplary embodiment, the weight fraction of PLA can also be 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts, 48 parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts and other typical but non-limiting weight fractions, or any number of parts between any two numerical ranges. Control the weight fraction of PLA within this range, and cooperate with components such as zinc oxide modified plant fiber to effectively improve the antibacterial properties of polylactic acid composite materials and improve the toughness and other mechanical properties of polylactic acid composite materials.
[0072] In some embodiments, PLA may include at least one of NatureWorks 4032D, Luminy LX175, and Fengyuan FY801. These PLAs have good thermal stability, so that the polylactic acid composite can be prepared by melting. At the same time, these PLAs have good degradability and can be effectively degraded by microorganisms in nature, thereby improving the degradability of the polylactic acid composite.
[0073] In some embodiments, the weight proportion of the copolymer of butylene adipate and butylene terephthalate [Poly (butylene adipate-co-terephthalate), PBAT] can be 10 to 30 parts, optionally 10 to 20 parts, 20 to 30 parts. In the exemplary embodiment, the weight proportion of PBAT can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc., which are typical but non-limiting weight proportions, or any proportion size between any two numerical ranges. PBAT has good biodegradability. By controlling the content of PBAT in the polylactic acid composite material within this range and compounding components such as PLA and zinc oxide-modified plant fiber, the toughness and impact resistance of the polylactic acid composite material can be further improved, and the tensile strength and elongation at break of the polylactic acid composite material can be improved.
[0074] In some embodiments, PBAT may include at least one of Tunhe TH801T, Huiyang HY-CM-6, and Sangosen L00022A. These PBATs have good degradability and excellent stable mechanical properties. These PBATs are compounded with components such as PLA to further improve the mechanical properties of polylactic acid composite materials.
[0075] In some embodiments, the weight proportion of polybutylene succinate [PBS] is 10 to 20 parts, and can be 10 to 15 parts, 15 to 20 parts. In the exemplary embodiment, the weight proportion of PBS can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc., which are typical but non-limiting weight proportions, or any proportion size between any two numerical ranges. PBS is a degradable plastic. By controlling the weight proportion of PBS within this range, the compounding of PBS with components such as PLA and zinc oxide modified plant fiber not only makes the polylactic acid composite material have good degradability, but also can effectively improve the mechanical properties of the tensile strength of the polylactic acid composite material.
[0076] In some embodiments, PBS may include at least one of Tunhe TH803S, Xuelang Technology BG211F1, and Thailand PTT Chemical FZ91PB. These PBSs have good mechanical properties, and these PBSs are compounded with PLA, zinc oxide modified plant fibers, etc. to further improve the toughness and other properties of polylactic acid composite materials.
[0077] In some embodiments, the polylactic acid composite material of the present application embodiment may further include an auxiliary agent, and the weight portion of the auxiliary agent may be 0.1 to 3 parts. In a further embodiment, the auxiliary agent may include at least one of a cross-linking agent, an antioxidant, and a compatibilizer. The addition of the auxiliary agent can promote the cross-linking between the molecular chains of the polylactic acid composite material, improve the compatibility between the components, further improve the mechanical properties such as toughness, and improve the anti-oxidation properties of the polylactic acid composite material.
[0078] In some embodiments, the polylactic acid composite material of the present application embodiment contains a crosslinking agent, and the weight portion of the crosslinking agent can be 0.1 to 1 part, and can be optionally 0.1 to 0.5 parts, 0.5 to 1 part. In the exemplary embodiment, the weight portion of the crosslinking agent can be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, etc. Typical but non-limiting weight portions, or any portion size between any two numerical ranges. By adding a crosslinking agent and controlling the weight portion of the crosslinking agent within this range, it is possible to promote crosslinking between polymer molecular chains such as polylactic acid, improve the compatibility of PLA with other components, further improve the mechanical properties of the polylactic acid composite material, and enhance the compressive strength.
[0079] In some embodiments, the crosslinking agent may include at least one of hydroquinone, peroxyacetylmalonate, and silane coupling agent KH550. These crosslinking agents have high reactivity, and by controlling the amount of the crosslinking agent added, the crosslinking density can be effectively controlled to enhance the mechanical properties of the polylactic acid composite material.
[0080] In some embodiments, the polylactic acid composite material of the present application embodiment contains an antioxidant, and the weight portion of the antioxidant can be 0.5 to 2 parts, and can be optionally 0.5 to 1 part, 1 to 2 parts. In the exemplary embodiment, the weight portion of the antioxidant can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, etc. Typical but non-limiting weight portions, or any portion size between any two numerical ranges. Controlling the weight portion of the antioxidant within this range effectively inhibits or reduces the thermal oxidation reaction rate of macromolecules in the polylactic acid composite material, improves the heat resistance of the polylactic acid composite material, and extends the service life of the polylactic acid composite material.
[0081] In some embodiments, the antioxidant may include at least one of antioxidant 1076, antioxidant 1010, and antioxidant 1135. These antioxidants have good compatibility with components such as PLA, good dispersibility in the polylactic acid composite material, stable effect, effectively extend the service life of the polylactic acid composite material, and reduce the impact on the mechanical properties of the polylactic acid composite material.
[0082] In some embodiments, the polylactic acid composite material of the present application embodiment also includes a compatibilizer, and the weight portion of the compatibilizer can be 0.5 to 2 parts, which can be selected as 0.5 to 1 part, 1 to 2 parts. In the exemplary example, the weight portion of the compatibilizer can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, etc. Typical but non-limiting weight portions, or any portion size between any two numerical ranges. Control the weight portion of the compatibilizer within this range, further improve the compatibility between PLA and components such as zinc oxide modified plant fiber, PBAT, PBS, and enhance the mechanical properties of the polylactic acid composite material. In the exemplary example, the compatibilizer can include at least one of dioctyl phthalate, epoxy furan resin, and di(2-ethylhexyl) phthalate.
[0083] In some embodiments, the polylactic acid composite material in the above embodiments may include the following components in parts by weight:
[0084]
[0085] By controlling the components such as PLA in the polylactic acid composite material within this range, the antibacterial properties of the polylactic acid composite material can be effectively improved, and the polylactic acid composite material can have good toughness, thereby effectively extending the service life of the polylactic acid composite material.
[0086] In some embodiments, in addition to the PBAT, PBS, antioxidant, cross-linking agent and compatibilizer mentioned above, the polylactic acid composite material of the embodiment of the present application may also include other components, such as masterbatch, etc., without specific limitation.
[0087] Based on the good antibacterial and mechanical properties of the polylactic acid composite material of the embodiment of the present application, the polylactic acid composite material of the embodiment of the present application can be applied to disposable or non-disposable plastic straws, water cups, packaging materials, and can also be applied to medical devices (such as infusion tubes, atomizing nozzles for nasal sprays, atomizers for drugs), electronic appliances, automotive parts, and sporting goods, without specific limitations.
[0088] In the second aspect, the present application provides a method for preparing a polylactic acid composite material. The polylactic acid composite material prepared by the method for preparing a polylactic acid composite material in the present application embodiment is the polylactic acid composite material mentioned above. The method for preparing a polylactic acid composite material in the present application embodiment comprises the following steps:
[0089] Step S10: mixing the raw materials including polylactic acid and zinc oxide modified plant fiber to obtain a polylactic acid mixture;
[0090] Step S20: melting the polylactic acid mixture to obtain a polylactic acid composite material.
[0091] The preparation method of the polylactic acid composite material of the embodiment of the present application is to melt the raw materials including polylactic acid and zinc oxide modified plant fiber, so that the polylactic acid composite material also contains zinc oxide. Compared with the zinc oxide particles attached to the surface of the polylactic acid material, the polylactic acid composite material prepared by the preparation method of the embodiment of the present application is more stably combined with the polylactic acid substrate. In addition, the preparation method of the embodiment of the present application attaches zinc oxide to the surface of the plant fiber and then mixes it with PLA, so that the mixing uniformity of the materials is better, the zinc oxide particles are not easy to aggregate and precipitate, and the stability of the obtained polylactic acid composite material is further improved.
[0092] Step S10:
[0093] In step S10, the raw materials including polylactic acid and zinc oxide modified plant fiber are mixed so that the raw materials are evenly mixed to obtain a polylactic acid mixture. The polylactic acid and zinc oxide modified plant fiber in step S10 are the polylactic acid and zinc oxide modified plant fiber mentioned above, which will not be described in detail.
[0094] In some embodiments, the mixed raw materials may also include the PBAT, PBA and cross-linking agent, antioxidant, and compatibilizer mentioned above, which will not be repeated here.
[0095] In some embodiments, the mixing process can be carried out in a high-speed mixer. The mixing speed can be 150 rpm, the temperature can be room temperature, and the time can be 30 minutes. There is no specific limitation, as long as the raw materials including polylactic acid and zinc oxide modified plant fiber are mixed evenly.
[0096] Step S20:
[0097] In step S20, the polylactic acid mixture is smelted to fully melt the polylactic acid and fully mix it with other components to obtain a polylactic acid composite material.
[0098] In some embodiments, the temperature of the smelting treatment can be 180-210°C, optionally 180-200°C, 190-210°C, 200-210°C. In the exemplary embodiment, the temperature of the smelting treatment can be typical but non-limiting temperatures such as 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, or any temperature between any two numerical ranges. Controlling the temperature of the smelting treatment within this range further promotes the melting of polymer components such as PLA and PBAT in the polylactic acid mixture, further improves the melt fluidity, promotes melt mixing, and improves the uniformity of the obtained polylactic acid composite material. In the exemplary embodiment, the operation of the smelting treatment can be to place the polylactic acid mixture in a twin-screw extruder for extrusion granulation, with an extrusion temperature of 180-210°C, a screw speed of 25rpm, and a feed rate of 15rpm.
[0099] In some embodiments, after the polylactic acid composite material is obtained through smelting treatment, the polylactic acid composite material can be further processed according to actual needs, such as drying, molding, etc., without specific limitation.
[0100] In order to enable the above implementation details and operations of the present application to be clearly understood by those skilled in the art, and to demonstrate the significant improvement in the performance of the polylactic acid composite material and the preparation method thereof in the embodiments of the present application, the above technical solution is illustrated by means of multiple embodiments below.
[0101] 1. Polylactic acid composite material and preparation method thereof
[0102] Example 1
[0103] This embodiment provides a polylactic acid composite material. The preparation method of the polylactic acid composite material in this embodiment includes the following steps:
[0104] Step S1: PLA, plant fiber, PBAT, PBS, crosslinking agent, antioxidant and compatibilizer are added to a high-speed mixer, and mixed at a speed of 150 rpm for 30 minutes at room temperature to obtain a polylactic acid mixture. The types and weight proportions of PLA, plant fiber, PBAT, PBS, crosslinking agent, antioxidant and compatibilizer used in the polylactic acid composite material of this embodiment are shown in Table 1.
[0105] Step S2: Add the polylactic acid mixture in step S1 into a twin-screw extruder for extrusion granulation, with an extrusion temperature of 180-210°C, a screw speed of 25 rpm, and a feed rate of 15 rpm. Dry the extruded masterbatch at 120°C for 12 hours to obtain the polylactic acid composite material of the present embodiment.
[0106] The plant fiber used in the preparation process of the polylactic acid composite material of this embodiment is zinc oxide modified plant fiber, and the zinc oxide modified plant fiber is prepared by a modification method comprising the following steps:
[0107] Step G1: Under room temperature, the plant fiber powder is dissolved in water and stirred at a speed of 200r / min. The plant fiber is bamboo fiber. After stirring evenly, the first alkali solution is added, wherein the first alkali solution is a 3wt% sodium hydroxide solution, and the ratio of the plant fiber to the first alkali solution is 1:30. Then, 0.5 parts of a dispersant (0.5wt% of the weight of the plant fiber) is added for alkali treatment for 12 hours. The dispersant is ethylenediaminetetraacetic acid. After the alkali treatment is completed, the plant fiber is separated, and the plant fiber is fully rinsed with water to neutrality, placed in a drying oven, and dried for 48 hours, so that the water content of the plant fiber is 5-8wt%, and the alkali-treated plant fiber is obtained.
[0108] Step G2: A 7 wt % zinc acetate dihydrate methanol solution was prepared, and the zinc acetate dihydrate methanol solution was mixed with a 0.03 mol / L monoethanolamine aqueous solution in a volume ratio of 1:1, and then stirred at 55° C. for 1 h using a magnetic stirrer until a uniform and stable colloidal solution was formed.
[0109] Step G3: Immerse the alkali-treated plant fiber obtained in step G1 in the colloidal solution obtained in the above step G2, take it out after one minute, and dry it at 80° C. for 2 hours to obtain pretreated plant fiber.
[0110] Step G4: Mix a 5wt% zinc acetate solution and a 3wt% sodium hydroxide solution in a volume ratio of 1:25 to obtain a precursor solution. Mix the pretreated plant fiber obtained in step G3 with the precursor solution and heat it in a polytetrafluoroethylene-lined autoclave at 135°C for 1h to perform a wet heat reaction. After the wet heat reaction, separate the plant fiber, rinse it with water ultrasonically for 30 minutes, and vacuum dry it at 50°C for 48h to obtain the zinc oxide-modified plant fiber used in the polylactic acid composite material of this embodiment.
[0111] Example 2 to Example 4
[0112] Embodiments 2 to 4 provide a polylactic acid composite material, respectively. The preparation methods of the polylactic acid composite materials in Embodiments 2 to 4 are substantially the same as the preparation method of the polylactic acid composite material in Embodiment 1, except that the PLA, plant fiber, PBAT, PBS, crosslinking agent, antioxidant and compatibilizer in the polylactic acid composite materials in Embodiments 2 to 4 are as shown in Table 1, and the preparation methods of zinc oxide-modified plant fibers in Embodiments 2 to 3 are different from the preparation methods of zinc oxide-modified plant fibers in Embodiment 1 as shown in Table 1, and the plant fibers in Embodiment 4 are not treated with alkali, but only with zinc oxide loading.
[0113] Comparative Example 1 to Comparative Example 3
[0114] Comparative Examples 1 to 3 provide a polylactic acid composite material, respectively. The preparation methods of the polylactic acid composite materials of Comparative Examples 1 to 3 are substantially the same as the preparation method of the polylactic acid composite material of Example 3, except that the PLA, plant fiber, PBAT, PBS, crosslinking agent, antioxidant and compatibilizer in the polylactic acid composite materials of Comparative Examples 1 to 3 are as shown in Table 1. Among them, the plant fiber of Comparative Example 1 is only subjected to alkali treatment and is not subjected to zinc oxide loading treatment, the plant fiber of Comparative Example 2 is neither subjected to alkali treatment nor subjected to zinc oxide loading treatment, and the plant fiber of Comparative Example 3 is the same as the plant fiber of Example 3.
[0115] Table 1
[0116]
[0117] 2. Performance Testing
[0118] The polylactic acid composite materials of Examples 1 to 4 and Comparative Examples 1 to 3 were dried at 120°C for 12 hours, and then subjected to tensile strength and elongation at break tests at a temperature of 25±1°C and a humidity of 50±5% RH, as well as antibacterial rate tests for Escherichia coli and Staphylococcus aureus. The results are shown in Table 2.
[0119] Among them, the test methods for tensile strength and elongation at break are determined by referring to GB / T13022-1991 Test method for tensile properties of plastic films; the antibacterial properties are determined by referring to GB / T 20944-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method".
[0120] Table 2
[0121]
[0122] As shown in Table 2, the polylactic acid composite materials of Examples 1 to 3 have high tensile strength and elongation at break, and also have good antibacterial effect on Escherichia coli and Staphylococcus aureus, with the antibacterial rate being above 99.99%. The plant fiber contained in the polylactic acid composite material of Example 4 was not subjected to alkali treatment, but directly loaded with zinc oxide. The polylactic acid composite material of Example 4 has good antibacterial effect, and its tensile strength and elongation at break are lower than those of the polylactic acid composite material of Example 3.
[0123] Compared with the polylactic acid composite material of Example 3, the plant fiber in the polylactic acid composite material of Comparative Example 1 was only treated with alkali, and no zinc oxide loading treatment was performed, and the antibacterial performance of the polylactic acid composite material of Comparative Example 1 was significantly reduced. Comparative Example 2 used plant fibers that were not treated with alkali and loaded with zinc oxide to prepare a polylactic acid composite material, and the antibacterial performance and toughness of the obtained polylactic acid composite material were significantly lower than those of the polylactic acid composite material of Example 3. The content of zinc oxide-modified plant fibers added to the polylactic acid composite material of Comparative Example 3 was higher than that of Example 3, and the tensile strength and elongation at break of the polylactic acid composite material of Comparative Example 3 were significantly lower than those of the polylactic acid composite material of Example 3.
[0124] Comparison of the tensile strength, elongation at break and antibacterial rate of the polylactic acid composite materials of the above-mentioned embodiments and comparative examples shows that the embodiments of the present application, by subjecting the plant fibers to specific alkali treatment and zinc oxide loading treatment and controlling the ratio of PLA and zinc oxide-modified plant fibers, make the compounding of zinc oxide-modified plant fibers and PLA and other materials effectively improve the antibacterial properties of the polylactic acid composite materials, while improving the toughness of the polylactic acid materials, and increasing the tensile strength and elongation at break of the polylactic acid materials.
[0125] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A polylactic acid composite material, It is characterized in that The polylactic acid composite material comprises the following components in parts by weight: Polylactic acid 40-60 parts 10-20 parts of zinc oxide modified plant fiber 0-30 parts of copolymer of butylene adipate and butylene terephthalate Polybutylene succinate 0-20 parts; The zinc oxide modified plant fiber comprises plant fiber and a zinc oxide coating layer, and the zinc oxide coating layer is coated on the surface of the plant fiber.
2. The polylactic acid composite material according to claim 1, It is characterized in that The zinc oxide coating layer includes at least one of the following (1) to (3): (1) The thickness of the zinc oxide coating layer is 0.5 to 1 μm; (2) The zinc oxide coating layer contains zinc oxide particles, and the particle size of the zinc oxide particles is 100 to 300 nm; (3) The coverage rate of the zinc oxide coating layer on the surface of the plant fiber is 60% to 80%.
3. The polylactic acid composite material according to claim 1, It is characterized in that The plant fiber includes at least one of bamboo fiber, balsa fiber and sisal fiber.
4. The polylactic acid composite material according to any one of claims 1 to 3, It is characterized in that The zinc oxide modified plant fiber is prepared by a modification method comprising the following steps: Using a first alkali solution to perform alkali treatment on the plant fiber to obtain alkali-treated plant fiber; placing the alkali-treated plant fiber in a colloidal solution containing zinc hydroxide particles for infiltration treatment to obtain pretreated plant fiber; The pretreated plant fiber is mixed with a precursor solution and subjected to a wet heat treatment to obtain the zinc oxide modified plant fiber.
5. The polylactic acid composite material according to claim 4, It is characterized in that The colloidal solution is prepared by a first stirring process of a first zinc salt solution and an organic base reagent; and / or The precursor solution is prepared by mixing a second zinc salt solution and a second alkali solution; and / or The temperature of the wet heat treatment is 130-150°C.
6. The polylactic acid composite material according to any one of claims 1 to 3 and 5, It is characterized in that The polylactic acid comprises at least one of NatureWorks4032D, LuminyLX175, and Fengyuan FY801; and / or The copolymer of butylene adipate and butylene terephthalate includes at least one of Tunhe TH801T, Huiyang HY-CM-6, and Sangosen L00022A; and / or The polybutylene succinate comprises at least one of Tunhe TH803S, Xuelang Technology BG211F1, and Thailand PTT Chemical FZ91PB; and / or The weight proportion of the copolymer of butylene adipate and butylene terephthalate is 10 to 30 parts; and / or The weight proportion of the polybutylene succinate is 10 to 20 parts; and / or The polylactic acid composite material comprises an auxiliary agent, and the weight proportion of the auxiliary agent is 0.1 to 3 parts.
7. The polylactic acid composite material according to claim 6, It is characterized in that The auxiliary agent includes a cross-linking agent, an antioxidant and a compatibilizer, and the weight proportions of the cross-linking agent, the antioxidant and the compatibilizer are as follows: Crosslinking agent 0.1~1 part Antioxidant 0.5-2 parts 0.5 to 2 parts of extender.
8. The polylactic acid composite material according to claim 7, It is characterized in that The cross-linking agent includes at least one of hydroquinone, peroxyacetylmalonate, and silane coupling agent KH550; The antioxidant includes at least one of antioxidant 1076, antioxidant 1010 and antioxidant 1135; The compatibilizer includes at least one of dioctyl phthalate, epoxy furan resin, and di(2-ethylhexyl) phthalate.
9. A method for preparing the polylactic acid composite material according to any one of claims 1 to 8, It is characterized in that The steps include: Mixing raw materials including the polylactic acid and the zinc oxide modified plant fiber to obtain a polylactic acid mixture; The polylactic acid mixture is subjected to smelting treatment to obtain the polylactic acid composite material.
10. The method according to claim 9, It is characterized in that The smelting process comprises the following steps: The polylactic acid mixture is extruded in a twin-screw extruder at a temperature of 180-210°C.