Oil-based plugging filtrate reducer and preparation method thereof
By combining graphene oxide with modified silica in oil-based drilling fluid fluid loss additives, and adding modified plant fiber and other ingredients to form a composite plugging structure, the existing technology solves the problem of high temperature leakage of fluid loss additives. The problem of insufficient temperature resistance has significantly improved the plugging effect and well wall stability.
Patent Information
- Application Number
- CN202410768895.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
AI Technical Summary
Existing oil-based drilling fluid fluid loss additives have insufficient temperature resistance at high temperatures, resulting in poor nano-micron plugging effect and inability to effectively reduce drilling fluid fluid loss and prevent well wall collapse.
By chemically combining graphene oxide with modified silica to enhance its thermal stability and water absorption properties, and adding modified plant fiber and (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt and 6-chlorotoluene-3-vinyl sulfonate to form a reversible network structure and agglomerated particles to achieve a composite blocking effect of points, surfaces and lines.
It significantly improves the heat resistance and mechanical properties of the fluid loss reducer, enhances the sealing effect on oil well fractures and nano-micron pores, reduces the fluid loss of drilling fluid and prevents well wall collapse.
Smart Images

Figure BDA0004893513340000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of oil drilling treatment agents, and in particular to an oil-based plugging and filtration reducer and a preparation method thereof. Background Art
[0002] At present, during the drilling process, due to the effect of pressure difference, the water in the drilling fluid will inevitably filter through the well wall into the formation, causing the drilling fluid to lose water. The working principle of the fluid loss reducer is to adsorb on the surface of the mud shale, block the pores, reduce the water absorption of the rock, and thus reduce the loss of drilling fluid. At the same time, they can also enhance the cohesion between shale particles, prevent the well wall from collapsing, and protect the stability of the well wall.
[0003] A Chinese invention patent with publication number CN115386349A discloses a plugging type fluid loss reducer for oil-based drilling fluid, comprising the following components and weight proportions: 8 to 12 parts of graphene oxide, 20 to 35 parts of attapulgite, 0.5 to 0.8 parts of initiator, 2 to 3 parts of silane coupling agent, 4 to 6 parts of cross-linking agent, 58 to 90 parts of matrix asphalt, and 11% calcium chloride solution, and 12 to 18 parts of polymerization monomer; the polymerization monomer is synthesized from acrylamide, acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid, wherein the weight ratio of acrylamide, acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid is 4:1:18.
[0004] Among them, graphene oxide has weak temperature resistance and is easily reduced at high temperatures, removing the oxygen-containing groups at the edge of the sheet, resulting in poor self-hydration performance and poor nano-micron sealing effect. Summary of the invention
[0005] In order to improve the temperature resistance of the fluid loss reducer and enhance the plugging effect, the present application provides an oil-based plugging fluid loss reducer and a preparation method thereof.
[0006] The present application provides a method for preparing an oil-based plugging and filtration reducer, which adopts the following technical scheme: A method for preparing an oil-based plugging and filtrate reducing agent comprises the following steps: S1: 0.5 to 1 parts by weight of graphene oxide, 8 to 12 parts by weight of water and 0.1 to 0.3 parts by weight of N-hydroxysuccinimide are mixed, and then 6 to 12 parts by weight of modified silicon dioxide are added, and mixed evenly to obtain a dispersion A; S2: 3-5 parts by weight of dispersion A, 1-3 parts by weight of modified plant fiber, 5-7 parts by weight of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt, 10-15 parts by weight of acrylamide, 8-10 parts by weight of 6-chlorotoluene-3-sulfonic acid vinyl ester, 1-3 parts by weight of polyethylene glycol, 2-4 parts by weight of a cross-linking agent, and 25-30 parts by weight of water are mixed, and the pH value is adjusted to 4-4.5, and then 0.03-0.07 parts by weight of an initiator is added, and the mixture is reacted at 50-60° C. for 4-6 hours, and dried to obtain a fluid loss reducer.
[0007] By adopting the above technical scheme, modified silicon dioxide is chemically bonded to the surface of graphene oxide. Therefore, silicon dioxide particles will not fall off from graphene oxide in subsequent polymer processing. Unique structural features can prevent the stacking (isolation effect of silicon dioxide particles) between graphene oxide sheets and the agglomeration of silicon dioxide particles (uniform growth on the graphene oxide surface, promoting uniform dispersion in the polymer matrix), and can significantly increase specific surface area, strengthen the interface bonding between the polymer. Because the graphene oxide surface has a large amount of oxygen-containing groups, such as carboxyl, hydroxyl, epoxy group, etc., carboxyl can carry out amide condensation with the amino group on the modified silicon dioxide surface, and then the graphene oxide sheet is coated on the silicon ball surface. The addition of N-hydroxysuccinimide can further activate the carboxyl group in graphene oxide, catalyze the carboxylamine reaction, and strengthen the bonding force between graphene oxide and silicon dioxide. The hybrid composite of graphene oxide and silicon dioxide can improve the water absorption performance of polyacrylamide, and enhance the thermal stability and mechanical properties of polyacrylamide. Due to its special structure, it can seal cracks and leaks in oil wells and enhance the sealing effect of nano-micron pores.
[0008] The addition of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt makes the hydrophobic part of polyacrylamide aggregate or associate in a similar way to surfactants, so that the effective flow size of the macromolecular coil is increased, and a reversible network structure is formed in the aqueous solution, which sharply increases the viscosity of the solution. The addition of 6-chlorotoluene-3-sulfonic acid vinyl ester can inhibit the oxidative degradation of the polymer chain and improve its heat resistance and salt resistance. Under the action of polyacrylamide, solid particles are prone to condensation, and modified plant fibers, as bridges, can provide a host for solid particles. When the fluid loss agent is added to the oil well and the fluid loss agent enters the oil well fracture channel, the solid particles quickly flocculate and squeeze out the water, leaving the modified plant fibers. This material is easy to deform and compress, and can fill the oil well fractures. In addition, the modified plant fibers, modified silica and graphene oxide are used in coordination to achieve point, surface and line three-item composite plugging of oil well fractures and improve the plugging effect.
[0009] Preferably, the preparation method of the modified silica comprises the following steps: mixing 0.3 to 0.6 parts by weight of γ-aminopropyltriethoxysilane with 10 to 15 parts by weight of ethanol solution, adjusting the pH to 4 to 5, hydrolyzing for 3 to 5 hours, adding 2 to 4 parts by weight of silica microspheres, reacting for 1 to 3 hours at 70 to 90° C., separating the solid from the liquid, washing and drying to obtain the modified silica.
[0010] By adopting the above technical solution, γ-aminopropyltriethoxysilane can react with the silanol groups on the surface of silica after hydrolysis, thereby enhancing the surface activity of silica, strengthening the adhesion, promoting the dispersibility of silica and improving the thermal stability of silica. The modified silica has little effect on the rheology of the drilling fluid, has good water loss wall-building properties, and has good plugging ability for nano-micropore formations.
[0011] Preferably, the particle size of the silica microspheres is 20 to 100 nm.
[0012] By adopting the above technical solution and optimizing the particle size of silica microspheres, the plugging effect of modified silica on nano-micropore formations can be further improved.
[0013] Preferably, the graphene oxide has a particle size of 10 to 20 μm.
[0014] By adopting the above technical solution and optimizing the particle size of graphene oxide, the blocking effect of graphene oxide on micron pores can be further improved.
[0015] Preferably, the cross-linking agent is water-soluble N,N'-methylenebisacrylamide.
[0016] By adopting the above technical solution, N,N'-methylenebisacrylamide contains two allyl double bonds, which can undergo addition reactions with other monomers or polymer segments containing nucleophilic reaction groups to form cross-linked structures, thereby achieving cross-linking of polymers. In addition, N,N'-methylenebisacrylamide is conducive to the stability of the system and the formation of microgels.
[0017] Preferably, the initiator is a compound of sodium bisulfite and persulfate, and the mass ratio of the sodium bisulfite to the persulfate is (0.02-0.04): (0.01-0.03).
[0018] By adopting the above technical solution, two substances with oxidizing and reducing properties are compounded, and free radicals are generated through redox reactions, thereby initiating monomer polymerization. The polymerization initiation speed is fast and the polymerization can be initiated at a relatively low temperature.
[0019] Preferably, the persulfate is one of sodium persulfate, potassium persulfate and ammonium persulfate.
[0020] Preferably, the method for preparing the modified plant fiber comprises the following steps: 1) 2 to 4 parts by weight of ramie fiber are mixed with 10 to 20 parts by weight of isopropanol solution, and then 3 to 5 parts by weight of sodium hydroxide solution are added, the temperature is raised to 60 to 80° C., the reaction is carried out for 30 to 50 minutes, the solid-liquid separation is performed, and the pretreated ramie fiber is obtained; 2) 1 to 3 parts by weight of the pretreated ramie fiber are mixed with 5 to 15 parts by weight of an isopropanol solution, and then 0.2 to 0.5 parts by weight of isopropyl trioleate titanate and 0.1 to 0.3 parts by weight of 3-butenetriethoxysilane are added, the pH value is adjusted to 4.0 to 4.5, and the mixture is immersed at 40 to 50° C. for 12 to 16 hours, washed and dried to obtain modified ramie fiber.
[0021] By adopting the above technical scheme, the isopropanol solution can increase the disorder of the fiber, which is beneficial to the sufficiency of the alkalization reaction. On the one hand, the hydroxide ions in the alkali solution will combine with the ester group in the fiber to form a hydroxyl group, which breaks the carbonyl group in the fiber molecule and decomposes it into smaller molecules. On the other hand, the hydroxide ions in the alkali solution can combine with the cations in the fiber molecule to neutralize its charge and dissociate it into smaller molecules. The addition of isopropyl trioleyl titanate can further improve the hydrophobicity and mechanical properties of the fiber. It can be used in conjunction with 3-butylene triethoxysilane to increase the crosslinking degree between fiber molecules.
[0022] The present application also provides an oil-based plugging and filtration reducer prepared by the above method.
[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. By compounding graphene oxide and modified silica, the heat resistance, adsorption performance and mechanical strength of polyacrylamide are improved, the cracks and leaks in the oil wells are blocked, and the blocking effect of nano-micron pores is enhanced.
[0024] 2. With the help of modified plant fibers as bridges, a host can be provided for solid particles. When the filtrate reducer is added to the oil well and enters the crack channel of the oil well, the solid particles quickly flocculate, squeezing out the water and leaving the modified plant fibers. This material is easy to deform and compress and can fill the cracks in the oil well. DETAILED DESCRIPTION
[0025] The present application is further described in detail below with reference to the embodiments.
[0026] Preparation Example 1-3 Preparation of modified plant fiber Preparation Example 1 The preparation method of the modified plant fiber in this preparation example comprises the following steps: 1) dispersing 3 kg of ramie fiber in 15 kg of 50% by mass isopropanol solution, then adding 5 kg of 0.5% by mass sodium hydroxide and stirring and mixing evenly, soaking for 40 minutes at 80° C., filtering, and then washing with distilled water and drying to obtain pretreated ramie fiber; 2) 2 kg of pretreated ramie fiber was mixed with 10 kg of 50% isopropanol solution by mass, and then 0.3 kg of isopropyl trioleate titanate and 0.2 kg of 3-butenetriethoxysilane were added, and the pH value was adjusted to 4.0 with glacial acetic acid. The mixture was soaked at 50 ° C for 12 h, and then washed with distilled water and dried until the solution was neutral. Finally, the mixture was placed in an oven and dried at 80 ° C for 6 h to obtain modified ramie fiber.
[0027] Preparation Example 2 The preparation method of the modified plant fiber in this preparation example comprises the following steps: 1) dispersing 2 kg of ramie fiber in 10 kg of 50% by mass isopropanol solution, then adding 3 kg of 0.5% by mass sodium hydroxide and stirring and mixing evenly, soaking for 30 minutes at 60° C., filtering, and then washing with distilled water and drying to obtain pretreated ramie fiber; 2) 1 kg of pretreated ramie fiber was mixed with 5 kg of 50% isopropanol solution by mass, and then 0.2 kg of isopropyl trioleate titanate and 0.3 kg of 3-butenetriethoxysilane were added, and the pH value was adjusted to 4.2 with glacial acetic acid. The mixture was soaked at 40 ° C for 16 h, and then washed with distilled water and dried until the solution was neutral. Finally, it was placed in an oven and dried at 80 ° C for 6 h to obtain modified ramie fiber.
[0028] Preparation Example 3 The preparation method of the modified plant fiber in this preparation example comprises the following steps: 1) dispersing 4 kg of ramie fiber in 20 kg of 50% by mass isopropanol solution, then adding 4 kg of 0.5% by mass sodium hydroxide and stirring and mixing evenly, soaking at 70° C. for 50 min, filtering, then washing with distilled water and drying to obtain pretreated ramie fiber; 2) 3 kg of pretreated ramie fiber was mixed with 15 kg of 50% isopropanol solution by mass, and then 0.5 kg of isopropyl trioleate titanate and 0.1 kg of 3-butenetriethoxysilane were added, and the pH value was adjusted to 4.5 with glacial acetic acid. The mixture was soaked at 45 ° C for 14 h, and then washed with distilled water and dried until the solution was neutral. Finally, it was placed in an oven and dried at 80 ° C for 6 h to obtain modified ramie fiber.
[0029] In other preparation examples, other reaction conditions and other amounts of ramie fiber, isopropyl alcohol, sodium hydroxide, isopropyl trioleate titanate, and 3-butenetriethoxysilane may be used, but the modified ramie fiber prepared may have poor effect.
[0030] Preparation Example 4-6 Preparation of modified silicon dioxide Preparation Example 4 The preparation method of modified silicon dioxide in this preparation example comprises the following steps: 0.5 kg of γ-aminopropyltriethoxysilane was mixed with 12 kg of 50% ethanol solution by mass, the pH was adjusted to 4.5 with glacial acetic acid, hydrolyzed for 4 hours, and then 3 kg of silica microspheres were added, reacted at 80° C. for 2 hours, filtered, washed, dried, and ground to obtain modified silica.
[0031] The particle size of the silica microspheres is 60 nm.
[0032] Preparation Example 5 The preparation method of modified silicon dioxide in this preparation example comprises the following steps: 0.3 kg of γ-aminopropyltriethoxysilane was mixed with 10 kg of 50% ethanol solution by mass, the pH was adjusted to 4 with glacial acetic acid, hydrolyzed for 3 hours, and then 2 kg of silica microspheres were added, reacted at 70° C. for 3 hours, filtered, washed, dried, and ground to obtain modified silica.
[0033] The particle size of the silica microspheres is 20 nm.
[0034] Preparation Example 6 The preparation method of modified silicon dioxide in this preparation example comprises the following steps: 0.6 kg of γ-aminopropyltriethoxysilane was mixed with 15 kg of 50% ethanol solution by mass, the pH was adjusted to 5 with glacial acetic acid, hydrolyzed for 5 hours, and then 4 kg of silica microspheres were added, reacted at 90° C. for 1 hour, filtered, washed, dried, ground and crushed to obtain modified silica.
[0035] The particle size of the silica microspheres is 100 nm.
[0036] In other preparation examples, other reaction conditions and other amounts of γ-aminopropyltriethoxysilane, ethanol, and silica microspheres may be used, but the modified silica prepared may have poor effects.
[0037] An embodiment of a method for preparing an oil-based plugging and fluid loss reducing agent of the present invention is as follows: Example 1 This embodiment provides a method for preparing an oil-based plugging and filtration reducer, comprising the following steps: S1: 1 kg of graphene oxide, 12 kg of deionized water and 0.3 kg of N-hydroxysuccinimide were mixed, ultrasonicated for 30 min, and then 6 kg of modified silica was added, ultrasonicated for 30 min and stirred for 1 h to mix well, to obtain dispersion A; S2: 5 kg of dispersion A, 6 kg of modified plant fiber, 7 kg of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt, 15 kg of acrylamide, 10 kg of 6-chlorotoluene-3-sulfonic acid vinyl ester, 4 kg of N,N'-methylenebisacrylamide, 3 kg of polyethylene glycol, and 30 kg of ionized water were mixed, and the pH was adjusted to 4.5 with NaOH, and then 30 g of potassium persulfate and 20 g of sodium bisulfite were added in sequence. The mixture was reacted at 60°C for 6 hours. After the reaction was completed, the mixture was dried in vacuum at 100°C to obtain a filtrate reducer.
[0038] The particle size of graphene oxide is 20 μm.
[0039] Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 1; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 4.
[0040] Example 2 This embodiment provides a method for preparing an oil-based plugging and filtration reducer, comprising the following steps: S1: 0.5 kg of graphene oxide, 8 kg of deionized water and 0.1 kg of N-hydroxysuccinimide were mixed, ultrasonicated for 30 min, and then 12 kg of modified silica was added, ultrasonicated for 30 min and stirred for 1 h to mix well, to obtain dispersion A; S2: 3 kg of dispersion A, 4 kg of modified plant fiber, 5 kg of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt, 10 kg of acrylamide, 8 kg of 6-chlorotoluene-3-sulfonic acid vinyl ester, 2 kg of N,N'-methylenebisacrylamide, 1 kg of polyethylene glycol, and 25 kg of ionized water were mixed, and the pH was adjusted to 4 with NaOH. Then, 10 g of sodium persulfate and 40 g of sodium bisulfite were added in sequence, and the reaction was carried out at 50°C for 4 hours. After the reaction was completed, vacuum drying was carried out at 100°C to obtain a filtrate reducer.
[0041] The particle size of graphene oxide is 15 μm.
[0042] Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 1; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 4.
[0043] Example 3 This embodiment provides a method for preparing an oil-based plugging and filtration reducer, comprising the following steps: S1: 0.8 kg of graphene oxide, 10 kg of deionized water and 0.2 kg of N-hydroxysuccinimide were mixed, ultrasonicated for 30 min, and then 8 kg of modified silica was added, ultrasonicated for 30 min and stirred for 1 h to mix well, to obtain dispersion A; S2: 4 kg of dispersion A, 5 kg of modified plant fiber, 6 kg of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt, 12 kg of acrylamide, 9 kg of 6-chlorotoluene-3-sulfonic acid vinyl ester, 3 kg of N,N'-methylenebisacrylamide, 2 kg of polyethylene glycol, and 27 kg of ionized water were mixed, and the pH was adjusted to 4.2 with NaOH, and then 20 g of ammonium persulfate and 30 g of sodium bisulfite were added in sequence, and the reaction was carried out at 55 ° C for 5 hours. After the reaction, vacuum drying was carried out at 100 ° C to obtain a filtrate reducer.
[0044] The particle size of graphene oxide is 10 μm.
[0045] Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 1; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 4.
[0046] Example 4 The difference between this embodiment and embodiment 3 is that: Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 2; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 5.
[0047] The rest is the same as in Example 3.
[0048] Example 5 The difference between this embodiment and embodiment 3 is that: Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 3; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 6.
[0049] The rest is the same as in Example 3.
[0050] Example 6 The difference between this embodiment and embodiment 3 is that: Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 1; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 5.
[0051] The rest is the same as in Example 3.
[0052] Example 7 The difference between this embodiment and embodiment 3 is that: Among them, the modified plant fiber is the modified plant fiber prepared in Preparation Example 1; and the modified silicon dioxide is the modified silicon dioxide prepared in Preparation Example 6.
[0053] The rest is the same as in Example 3.
[0054] Comparative Example 1 The difference between this comparative example and Example 6 is that: S1: 0.8 kg of graphene oxide, 10 kg of deionized water and 0.2 kg of N-hydroxysuccinimide were mixed, and ultrasonicated for 30 min and stirred for 1 h until the mixture was uniform, to obtain dispersion A; The rest is the same as Example 6.
[0055] Comparative Example 2 The difference between this comparative example and Example 6 is that: S1: 8 kg of modified silica, 10 kg of deionized water and 0.2 kg of N-hydroxysuccinimide were mixed, and ultrasonicated for 30 min and stirred for 1 h until the mixture was uniform, to obtain dispersion A; The rest is the same as Example 6.
[0056] Comparative Example 3 The difference between this comparative example and Example 6 is that: S1: 0.8 kg of graphene oxide, 10 kg of deionized water and 0.2 kg of N-hydroxysuccinimide were mixed, ultrasonicated for 30 min, and then 8 kg of silicon dioxide was added, ultrasonicated for 30 min and stirred for 1 h to mix well, to obtain dispersion A; The rest is the same as Example 6.
[0057] Comparative Example 4 The difference between this comparative example and Example 6 is that dispersion A is not added.
[0058] The rest is the same as Example 6.
[0059] Comparative Example 5 The difference between this comparative example and Example 6 is that the plant fiber is not modified.
[0060] Experimental example Performance Testing (1) Preparation of base slurry Add 100g calcium bentonite and 5g anhydrous sodium carbonate into 2500ml clean water, stir at high speed for 30min, and let stand for 24h for use.
[0061] 1. Fluid loss agent performance test: Add different mass fractions of fluid loss agents into the base slurry and stir at 8000 rpm for 30 minutes. The mixture was loaded into an aging tank and placed in a roller furnace. It was rolled at 120°C for 16 hours, taken out and cooled to room temperature, and then stirred at 8000 rpm for 20 minutes. Its rheological properties and filtration loss performance were measured using a ZNN-D6 six-speed rotational viscometer and a GGS71-A high-temperature and high-pressure filtration loss tester. The results are shown in Table 1.
[0062] An example of performance test of an oil-based plugging and fluid loss reducer of the present invention is as follows: Example 8 Take 1 g of the filtration reducer prepared in Example 1, add it to 100 ml of the base slurry, stir it at 8000 rpm for 30 min, put it into an aging tank, put it into a roller furnace, roll it at 120°C for 16 h, take it out and cool it to room temperature, stir it at 8000 rpm for 20 min, and measure its rheological properties and filtration loss performance.
[0063] Example 9 Take 2 g of the filtration reducer prepared in Example 1, add it to 100 ml of the base slurry, stir it at 8000 rpm for 30 min, put it into an aging tank, put it into a roller furnace, roll it at 120°C for 16 h, take it out and cool it to room temperature, stir it at 8000 rpm for 20 min, and measure its rheological properties and filtration loss performance.
[0064] Example 10 Take 3 g of the filtration reducer prepared in Example 1, add it to 100 ml of the base slurry, stir it at 8000 rpm for 30 min, put it into an aging tank, put it into a roller furnace, roll it at 120°C for 16 h, take it out and cool it to room temperature, stir it at 8000 rpm for 20 min, and measure its rheological properties and filtration loss performance.
[0065] Examples 11-14 Take 2 g of the filtration reducer prepared in Examples 2-5, add them to 100 ml of base slurry respectively, stir at 8000 rpm for 30 min, put them into an aging tank, put them into a roller furnace, roll them at 120°C for 16 h, take them out and cool them to room temperature, stir them at 8000 rpm for 20 min, and measure their rheological properties and filtration loss properties respectively.
[0066] Examples 15-16 Take 2 g of the filtration reducer prepared in Examples 6-7, add them to 100 ml of base slurry respectively, stir at 8000 rpm for 30 min, put them into an aging tank, put them into a roller furnace, roll them at 120°C for 16 h, take them out and cool them to room temperature, stir them at 8000 rpm for 20 min, and measure their rheological properties and filtration loss properties respectively.
[0067] Comparative Examples 6-10 Take 2g of the filtration reducer prepared in Comparative Examples 1-5, add them into 100ml of base slurry respectively, stir at 8000rpm for 30min, put them into aging tank, put them into a roller furnace, roll them at 120℃ for 16h, take them out and cool them to room temperature, stir them at 8000rpm for 20min, and measure their rheological properties and filtration loss properties respectively.
[0068] Table 1 Test results of Examples 8-16 and Comparative Examples 6-10 By analyzing and comparing Examples 8 to 10, it is found that when the amount of polyacrylamide added to 100 ml of mud is 2 g, a better filtration effect can be achieved, meeting the needs of practical applications. If the viscosity of the mud is too high, additives such as viscosity reducers need to be added to avoid oil well blockage.
[0069] By comparing and analyzing Examples 9 and 11 to 16, it is found that Example 6 has the best filtration effect, which may be due to the small particle sizes of the modified silica and graphene oxide in the dispersion. Smaller particles have a larger specific surface area and higher activity, and have a stronger interaction with the polymer, resulting in a higher enhancement effect. The porous water absorption characteristics of the modified plant fiber coat the silica nanoparticles and graphene oxide sheets dispersed in the water on the surface of the plant fiber, achieving a three-dimensional plugging effect of points, sheets, and lines.
[0070] A comparative analysis of Example 15 and Comparative Examples 6-10 shows that when graphene oxide or modified silica is used alone or no dispersion is added, the blocking effect of the polymer is poor; when unmodified plant fibers are used, due to their low bending strength and weak adsorption, when they are compounded with polymers and solid phase particles, the interfacial tension is large and the bonding strength is weak, resulting in varying degrees of decrease in their mechanical properties, thereby reducing the blocking effect.
Claims
1. A method for preparing an oil-based plugging and filtration reducer, characterized in that: The steps include: S1: 0.5-1 parts by weight of graphene oxide, 8-12 parts by weight of water and 0.1-0.3 parts by weight of N-hydroxysuccinimide are mixed, and then 6-12 parts by weight of modified silicon dioxide are added, and mixed evenly to obtain a dispersion A; S2: 3-5 parts by weight of dispersion A, 1-3 parts by weight of modified plant fiber, 5-7 parts by weight of (Z)-9-octadecenoic acid-2-sulfoethyl ester sodium salt, 10-15 parts by weight of acrylamide, 8-10 parts by weight of 6-chlorotoluene-3-sulfonic acid vinyl ester, 1-3 parts by weight of polyethylene glycol, 2-4 parts by weight of a cross-linking agent, and 25-30 parts by weight of water are mixed, the pH value is adjusted to 4-4.5, and then 0.03-0.07 parts by weight of an initiator is added, and the mixture is reacted at 50-60°C for 4-6 hours, and dried to obtain a fluid loss reducer.
2. The method for preparing the oil-based plugging and filtration reducer according to claim 1, characterized in that: The preparation method of the modified silicon dioxide comprises the following steps: mixing 0.3-0.6 parts by weight of γ-aminopropyltriethoxysilane with 10-15 parts by weight of ethanol solution, adjusting the pH to 4-5, hydrolyzing for 3-5 hours, adding 2-4 parts by weight of silicon dioxide microspheres, reacting for 1-3 hours at 70-90° C., separating the solid from the liquid, washing and drying to obtain the modified silicon dioxide.
3. The method for preparing the oil-based plugging and filtration reducer according to claim 2, characterized in that: The particle size of the silica microspheres is 20-100 nm.
4. The method for preparing the oil-based plugging and filtration reducer according to claim 1, characterized in that: The graphene oxide particle size is 10-20 μm.
5. The method for preparing the oil-based plugging and filtration reducer according to claim 1, characterized in that: The cross-linking agent is water-soluble N,N'methylenebisacrylamide.
6. The method for preparing the oil-based plugging and filtration reducer according to claim 1, characterized in that: The initiator is prepared by compounding sodium bisulfite and persulfate, and the mass ratio of the sodium bisulfite to the persulfate is (0.02-0.04): (0.01-0.03).
7. The method for preparing the oil-based plugging and filtration reducer according to claim 1, characterized in that: The method for preparing the modified plant fiber comprises the following steps: 1) 2-4 parts by weight of ramie fiber and 10-20 parts by weight of isopropanol solution are mixed, then 3-5 parts by weight of sodium hydroxide solution are added, the temperature is raised to 60-80° C., the reaction is carried out for 30-50 minutes, solid-liquid separation is performed, washing and drying are performed, and pretreated ramie fiber is obtained; 2) 1-3 parts by weight of the pretreated ramie fiber is mixed with 5-15 parts by weight of an isopropanol solution, and then 0.2-0.5 parts by weight of isopropyl trioleate titanate and 0.1-0.3 parts by weight of 3-butenetriethoxysilane are added, the pH value is adjusted to 4.0-4.5, and the mixture is immersed at 40-50°C for 12-16 hours, washed and dried to obtain modified ramie fiber.
8. An oil-based plugging and filtration reducer prepared by the method according to claims 1 to 7.
Citation Information
Cited By
Well drilling plugging agent as well as preparation method and application thereof
CN121780143A
A well drilling plugging agent, its preparation method and application
CN121780143B