Solid electrolyte and preparation method thereof, electrolyte membrane and battery
By using a combination method of polymer, lithium salt and ceramic powder in solid-state lithium batteries, and modifying the electrode interface with the second lithium salt, the low conductivity and short life of the solid-state electrolyte are solved, and high The stability and cycling performance of energy density batteries are improved.
Patent Information
- Application Number
- CN202410960881.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The solid electrolytes of existing solid-state lithium batteries have low ionic conductivity and limited electrochemical stability windows under room temperature conditions, resulting in short cycle life, especially under high energy density positive electrodes, which can easily cause side reactions, affecting battery performance.
Using a combination method of polymer, first lithium salt, nitrogen-containing crosslinking agent and ceramic powder, a three-dimensional network structure is formed by heating curing, which improves the ionic conductivity of the solid electrolyte, and modifies the electrode interface through the second lithium salt to reduce the secondary reaction.
It significantly improves the room temperature ionic conductivity and cycling stability of solid electrolytes, extends the cycle life of the battery, and is suitable for applications with high energy density batteries.
Smart Images

Figure CN118919824A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium batteries, and in particular, relates to a solid electrolyte and a preparation method thereof, an electrolyte membrane and a battery. Background Art
[0002] The organic solvents in liquid lithium-ion batteries are volatile and flammable, making it difficult to effectively guarantee the safety performance and high energy density of liquid lithium-ion batteries. At the same time, organic solvents are very easy to decompose under high voltage, and continue to react with electrodes during the battery cycle, causing the overall performance of the battery to decay rapidly. Compared with liquid lithium-ion batteries, solid-state lithium batteries have higher safety and energy density. As the core component of solid-state lithium batteries, solid electrolytes determine the performance level of solid-state lithium batteries. Among them, organic-inorganic solid electrolytes have comprehensive advantages in electrochemical properties, mechanical properties and processing difficulty compared to single-component electrolytes, and therefore have received extensive attention and research.
[0003] Among the existing organic-inorganic solid electrolyte systems, ceramic / polymer solid electrolytes (hereinafter referred to as solid electrolytes) are expected to achieve practical applications in solid-state lithium batteries. However, the current mainstream solid electrolytes have complex preparation and processing processes, and Li + Low conductivity, limited electrochemical stability window and other issues. In particular, in order to reveal the true potential of solid-state lithium batteries in the field of high energy density, it is necessary to adapt to a cut-off voltage greater than 4.3V vs. Li + / Li high energy density positive electrode (cathode). At such a high potential level, the organic matrix of most solid electrolytes, such as polyethylene oxide (PEO) and polyvinyl carbonate (PEC), are unstable. Especially under the high pressure oxygen release of common layered positive electrodes, such as lithium cobalt oxide (LiCoO2) and high nickel positive electrodes and the oxidation catalysis of transition metal ions, the solid electrolyte matrix is very prone to continuous irreversible side reactions, resulting in the consumption of lithium in the electrolyte and the failure of electrolyte components and structures. In addition, the existing solid electrolytes have poor modification of the electrode interface, which has a great negative impact on the cycle life of the battery.
[0004] Therefore, how to improve the ionic conductivity of solid electrolytes at room temperature so that the battery has higher cycle stability is a technical problem to be solved. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a solid electrolyte and a preparation method thereof, a solid electrolyte membrane and a battery. The solid electrolyte obtained by the method of the present application has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0006] In the first aspect of the present invention, the present invention proposes a method for preparing a solid electrolyte. According to an embodiment of the present invention, the preparation method includes: mixing a polymer, a first lithium salt, a nitrogen-containing crosslinking agent and a solvent, heating and curing to obtain an organic matrix, wherein the polymer contains a polyethylene glycol segment; mixing the organic matrix, a second lithium salt and a ceramic powder to obtain a solid electrolyte.
[0007] According to the preparation method of the above embodiment of the present invention, the polymer containing polyethylene glycol segments is mixed with the first lithium salt and the nitrogen-containing cross-linking agent for heat curing, wherein the ether oxygen group in the polyethylene glycol segment can be used as a hydrogen bond acceptor, and the nitrogen-containing cross-linking agent can be used as a hydrogen bond donor, so that the polyethylene glycol segment and the nitrogen-containing cross-linking agent can form hydrogen bonds, realize physical cross-linking between polymer chains, and then form a three-dimensional network structure. The lithium ions provided by the first lithium salt can form coordination bonds with the oxygen atoms in the polyethylene glycol segment, thereby promoting the dissociation of the first lithium salt and generating directional conduction through the movement of the segments, thereby improving the ionic conductivity of the solid electrolyte, which is beneficial to improving the ionic conductivity of the solid electrolyte. Moreover, during the process of heating and curing, the physical cross-linking points gradually stabilize, forming a more solid three-dimensional network, which can improve the stability of the solid electrolyte, and then help improve the cycle stability of the solid-state battery. Further, the organic matrix, the second lithium salt and the ceramic powder are mixed, wherein the addition of the second lithium salt can further provide lithium ions, improve the ionic conductivity of the solid electrolyte, and in the charge and discharge process of the solid-state battery, the inorganic and organic components produced by the decomposition of the second lithium salt can modify the electrode interface, promote the formation and stability of the electrode interface phase, thereby reducing side reactions and further improving the cycle stability of the solid-state battery. Ceramic powder can form a mixed conductor with an organic matrix, utilize the ionic conductivity of ceramics, realize the ion transmission of the solid electrolyte, and then improve the ionic conductivity of the solid electrolyte. Ceramic powder can also be used as rigid particles, dispersed in the organic matrix of the solid electrolyte, and can be used as a reinforcement to improve the mechanical properties of the solid electrolyte. Thus, the solid electrolyte obtained by the method provided by the present application has a higher ionic conductivity, and can modify the electrode interface, which is conducive to improving the cycle stability of the battery.
[0008] In addition, the preparation method according to the above embodiment of the present invention may also have the following additional technical features:
[0009] In some embodiments of the present invention, the polyethylene glycol segment in the polymer includes a repeating unit -CH2CH2O-, and the molar ratio of the repeating unit -CH2CH2O- to the lithium ions in the first lithium salt is (5-20): 1. Thus, the excess of lithium ions can be limited, the risk of lithium dendrite formation can be avoided, and the cycle stability of the solid-state battery can be improved.
[0010] In some embodiments of the present invention, the number average molecular weight of the polymer is 200 to 1000. Thus, the mobility of the polymer chain segments can be increased, which is beneficial to improving the mobility of lithium ions, thereby improving the ionic conductivity of the solid electrolyte.
[0011] In some embodiments of the present invention, the polymer includes at least one of polyethylene glycol and polyethylene glycol dimethyl ether, thereby forming a three-dimensional network structure and forming a coordination bond with the first lithium salt to enhance the conductivity of lithium ions, which is beneficial to improving the ionic conductivity of the solid electrolyte.
[0012] In some embodiments of the present invention, the first lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium perchlorate. Thus, the obtained solid electrolyte has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0013] In some embodiments of the present invention, the nitrogen-containing crosslinking agent accounts for 5% to 15% of the mass of the polymer. This is beneficial to improving the stability of the solid electrolyte, thereby improving the cycle stability of the solid-state battery.
[0014] In some embodiments of the present invention, the cross-linking agent includes N,N'-methylenebisacrylamide, which is beneficial to improve the stability of the solid electrolyte and thus improve the cycle stability of the solid-state battery.
[0015] In some embodiments of the present invention, the curing temperature is 80° C. to 100° C. This can promote the mobility of polymer molecular segments and facilitate the interaction and diffusion between the crosslinking agent and the polymer molecules.
[0016] In some embodiments of the present invention, the curing time is 30 minutes to 60 minutes, so that the physical crosslinking between the nitrogen-containing crosslinking agent and the polymer containing the polyethylene glycol segment reaches a high degree of completion, and a stable three-dimensional polymer network structure can be formed.
[0017] In some embodiments of the present invention, the second lithium salt accounts for 20% to 40% of the molar amount of the first lithium salt. Thus, the obtained solid electrolyte has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0018] In some embodiments of the present invention, the second lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate, and lithium tetrafluoroborate, thereby improving the cycle stability of the solid-state battery.
[0019] In some embodiments of the present invention, based on the total mass of the organic matrix and the ceramic powder, the mass of the ceramic powder accounts for 60% to 80%. Thus, the obtained solid electrolyte has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0020] In some embodiments of the present invention, the ceramic powder includes at least one of a first ceramic powder and a second ceramic powder, wherein the first ceramic powder includes at least one of lithium lanthanum zirconium tantalum oxide, lithium tantalum phosphate, lithium aluminum titanium phosphide and lithium lanthanum titanium oxide; and the second ceramic powder includes at least one of aluminum oxide, zirconium oxide and silicon oxide. Thus, the ionic conductivity of the solid electrolyte can be improved and the mechanical properties of the solid electrolyte can be improved.
[0021] In some embodiments of the present invention, the average particle size Dv50 of the first ceramic powder is 50 nm-1000 nm, which is beneficial to improve the ionic conductivity of the solid electrolyte and the cycle stability of the solid-state battery.
[0022] In some embodiments of the present invention, the average particle size Dv50 of the second ceramic powder is 0.1 μm-1 μm, which is beneficial to improve the ionic conductivity of the solid electrolyte and the cycle stability of the solid-state battery.
[0023] In a second aspect of the present invention, the present invention provides a solid electrolyte, and according to an embodiment of the present invention, the solid electrolyte is prepared by the above method. The solid electrolyte has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the solid-state battery.
[0024] In the third aspect of the present invention, the present invention provides a solid electrolyte membrane according to an embodiment of the present invention, wherein the solid electrolyte membrane comprises the solid electrolyte of the second aspect. The solid electrolyte membrane has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the solid-state battery.
[0025] In the fourth aspect of the present invention, a battery is proposed. According to an embodiment of the present application, the battery includes the solid electrolyte membrane of the third aspect, which has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0026] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0028] Figure 1 SEM micrographs of the solid electrolyte membrane of Example 1 are shown, wherein (a) is a surface SEM photograph; (b) is a cross-sectional SEM photograph;
[0029] Figure 2 A digital photograph of the solid electrolyte membrane of Example 1 is shown;
[0030] Figure 3 The graph shows the temperature-dependent ionic conductivity of the solid electrolyte of Example 1;
[0031] Figure 4 shows the LSV test diagram of the solid electrolyte of Example 1 at room temperature;
[0032] Figure 5 The long cycle discharge specific capacity-Coulomb efficiency of the battery of Example 1 at 30°C and 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.45V;
[0033] Figure 6 The long cycle discharge specific capacity-Coulomb efficiency of the battery of Example 1 at 30°C and 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.6V;
[0034] Figure 7 The specific capacity-voltage change of the battery of Example 1 during the long cycle at 30°C and 0.5C is shown, and the cycle cut-off voltage range is 3.0 to 4.45V;
[0035] Figure 8 The figure shows the rate performance of the battery of Example 1 at 30°C and different cut-off voltage ranges, where (a) the cut-off voltage is 4.45V; (b) the cut-off voltage is 4.6V;
[0036] Fig. 9 The SEM images of the positive electrode (a) and negative electrode (b) surface morphologies of the battery of Example 1 after 5 cycles at 0.2C and the corresponding EDS element distributions on the positive electrode (c) and negative electrode (b) surfaces are shown. The inset in Figure (a) is the original LCO positive electrode surface morphology;
[0037] Fig.10 The XPS spectrum of the negative electrode surface of the battery of Example 1 after 5 cycles at 0.2C is shown;
[0038] Fig.11 The XPS comparison of the positive electrode surface of the battery of Example 1 before and after 5 cycles at 0.2C is shown;
[0039] Fig.12The long cycle discharge specific capacity-Coulomb efficiency of the battery of Comparative Example 2 at 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.6V;
[0040] Fig.13 The specific capacity-voltage variation of the battery of Example 2 during a long cycle at 0.5C is shown, and the cycle cut-off voltage range is 3.0 to 4.6V. DETAILED DESCRIPTION
[0041] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0042] In a first aspect of the present invention, the present invention provides a method for preparing a solid electrolyte. According to an embodiment of the present invention, the preparation method comprises:
[0043] S1. Mixing a polymer, a first lithium salt, a nitrogen-containing crosslinking agent and a solvent, and heating and curing the mixture to obtain an organic matrix, wherein the polymer contains a polyethylene glycol segment.
[0044] In this step, after mixing the polymer containing polyethylene glycol segments with the first lithium salt and the nitrogen-containing crosslinking agent, heat curing is performed, wherein the ether radical in the polyethylene glycol segments can be used as a hydrogen bond acceptor, and the nitrogen-containing crosslinking agent can be used as a hydrogen bond donor, so that hydrogen bonds can be formed between the polyethylene glycol segments and the nitrogen-containing crosslinking agent, physical crosslinking between polymer chains can be achieved, and a three-dimensional network structure can be formed. The lithium ions decomposed by the first lithium salt can form coordination bonds with the oxygen atoms in the polyethylene glycol segments, be fixed in the three-dimensional network structure, and achieve ion conduction, which is conducive to improving the ionic conductivity of the solid electrolyte. Moreover, during the heat curing process, the physical crosslinking points gradually stabilize, forming a more solid three-dimensional network, which can improve the stability of the organic matrix, and thus help improve the cycle stability of the solid-state battery, thereby, an organic matrix with better stability can be obtained.
[0045] It should be noted that the mixing method is not particularly limited. According to a specific embodiment of the present invention, the polymer, the first lithium salt and the nitrogen-containing crosslinking agent are mixed by magnetic stirring to completely dissolve the first lithium salt and the nitrogen-containing crosslinking agent in the polymer.
[0046] According to some specific embodiments of the present invention, magnetic stirring is used as an aid during the heating and curing process to increase the contact frequency between reactants, accelerate the cross-linking or dissolution process, and thus increase the curing rate.
[0047] According to some specific embodiments of the present invention, the polyethylene glycol segment in the polymer includes a repeating unit -CH2CH2O-, and the molar ratio of the repeating unit -CH2CH2O- to the lithium ions in the first lithium salt is (5-20):1. For example, it can be 5:1, 10:1, 15:1, 20:1, etc. By limiting the molar ratio of the repeating unit -CH2CH2O- to the lithium ions in the first lithium salt to the above range, the polyethylene glycol segment can provide more oxygen atoms to form coordination bonds with lithium ions, thereby increasing the dissociation degree of the first lithium salt, thereby increasing the concentration of free lithium ions, which is beneficial to improving the ionic conductivity of the solid electrolyte.
[0048] According to some specific embodiments of the present invention, the first lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium perchlorate (LiClO4). By selecting the above-mentioned first lithium salt, a large number of free lithium ions are dissociated in the polymer matrix through dissolution and complexation, which is beneficial to improve the ionic conductivity of the solid electrolyte.
[0049] According to some specific embodiments of the present invention, the number average molecular weight (M n ) is 200 to 1000. For example, it can be 200, 500, 800, 1000, etc. By limiting the number average molecular weight of the polymer to the above range, the mobility of the polymer chain segment can be increased, which is beneficial to improving the mobility of lithium ions, thereby improving the ionic conductivity of the solid electrolyte.
[0050] According to some specific embodiments of the present invention, the polymer includes at least one of polyethylene glycol (PEG) and polyethylene glycol dimethyl ether (PEGDME). Both polyethylene glycol and polyethylene glycol dimethyl ether contain ether radicals, which can serve as hydrogen bond receptors, can form hydrogen bonds with nitrogen-containing crosslinking agents, achieve physical crosslinking between polymer chains, and further form a three-dimensional network structure, and can also form coordination bonds with the first lithium salt to enhance the conductivity of lithium ions, which is beneficial to improving the ionic conductivity of the solid electrolyte.
[0051] According to some specific embodiments of the present invention, the cross-linking agent accounts for 5% to 15% of the mass of the polymer. For example, it can be 5%, 8%, 10%, 13%, 15%, etc. By limiting the content of the cross-linking agent within the above range, the cross-linking agent can effectively connect the polymer chains to form a three-dimensional network structure without excessive cross-linking causing the material to become brittle. As a result, it is beneficial to improve the stability of the solid electrolyte, thereby improving the cycle stability of the solid-state battery.
[0052] According to some specific embodiments of the present invention, the cross-linking agent includes N,N'-methylenebisacrylamide (MBAM). The amide group (-CONH-) in N,N'-methylenebisacrylamide acts as a hydrogen bond donor and can form hydrogen bonds with polyethylene glycol segments to achieve physical cross-linking between polymer chains, thereby forming a three-dimensional network structure, improving the stability of the solid electrolyte, and thus facilitating the improvement of the cycle stability of the solid-state battery.
[0053] According to some specific embodiments of the present invention, the curing temperature is 80° C. to 100° C. For example, it can be 80° C., 90° C., 100° C., etc. By limiting the curing temperature to the above range, the mobility of the polymer molecular segments can be promoted, which is conducive to the interaction and diffusion between the crosslinking agent and the polymer molecules.
[0054] According to some specific embodiments of the present invention, the curing time is 30 minutes to 60 minutes. For example, it can be 30 minutes, 40 minutes, 50 minutes, 60 minutes, etc. By limiting the curing time within the above range, the physical crosslinking between the nitrogen-containing crosslinking agent and the polymer containing the polyethylene glycol segment can reach a higher degree of completion, and a stable three-dimensional polymer network structure can be formed.
[0055] S2. Mixing an organic matrix, a second lithium salt and a ceramic powder to obtain a solid electrolyte.
[0056] In this step, the organic matrix, the second lithium salt and the ceramic powder are mixed. Specifically, the organic matrix, the second lithium salt and the ceramic powder are placed in a mixing tank and sealed, and a vibrating ball mill or a high-speed centrifugal homogenizer is used to mix the organic matrix and the ceramic powder to form a uniform solid electrolyte block. Wherein, the addition of the second lithium salt can further provide lithium ions and improve the ionic conductivity of the solid electrolyte. At the same time, during the charge and discharge process of the solid-state battery, the inorganic and organic components produced by the decomposition of the second lithium salt can modify the electrode interface, promote the formation and stability of the electrode interface phase, thereby reducing side reactions and further improving the cycle stability of the solid-state battery. Ceramic powder can form a mixed conductor with the organic matrix, and the ionic conductivity of the ceramic and the electronic insulation of the organic material are used to realize the ion transmission of the solid electrolyte, thereby improving the ionic conductivity of the solid electrolyte. Ceramic powder can also be used as rigid particles, dispersed in the organic matrix of the solid electrolyte, and can be used as a reinforcement to improve the mechanical properties of the solid electrolyte.
[0057] According to some specific embodiments of the present invention, the second lithium salt accounts for 20% to 40% of the molar amount of the first lithium salt. For example, it can be 20%, 30%, 40%, etc. The main function of the second lithium salt is to act as an interface stabilizer. If the content of the second lithium salt is too little, the electrode interface stability problem cannot be completely solved; if the content of the second lithium salt is too much, it will cause an increase in cost. Therefore, by limiting the amount of the second lithium salt to be added within the above range, the obtained solid electrolyte has a higher ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0058] As an example, the second lithium salt includes but is not limited to at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorooxalate borate (LiDFOB), lithium perchlorate (LiClO4), and lithium tetrafluoroborate (LiTFB). By selecting the above-mentioned second lithium salt, additional lithium ions can be provided, which helps to increase the lithium ion concentration in the solid electrolyte, thereby improving the ionic conductivity of the solid electrolyte. At the same time, during the charge and discharge process of the solid-state battery, the inorganic and organic components produced by the decomposition of the second lithium salt can modify the electrode interface and form a stable SEI film, thereby reducing side reactions and further improving the cycle stability of the solid-state battery. Furthermore, the second lithium salt includes at least one of lithium difluorooxalate borate and lithium tetrafluoroborate.
[0059] According to some specific embodiments of the present invention, based on the total mass of the organic matrix and the ceramic powder, the mass proportion of the ceramic powder is 60% to 80%. For example, it can be 60%, 70%, 80%, etc. If the mass proportion of the ceramic powder is too small, the electrolyte film forming effect will be poor and the mechanical strength will be low. If the mass proportion of the ceramic powder is too high, the electrolyte will crack and cause huge interface resistance. Therefore, by limiting the mass proportion of the ceramic powder to the above range, the obtained solid electrolyte has a higher ionic conductivity and can modify the electrode interface, which is beneficial to improve the cycle stability of the battery.
[0060] According to some specific embodiments of the present invention, the ceramic powder includes at least one of a first ceramic powder and a second ceramic powder, wherein the first ceramic powder includes at least one of lithium lanthanum zirconium tantalum oxide (LLZTO), lithium tantalum phosphate (LTPO), lithium aluminum titanium phosphide (LATP), and lithium lanthanum titanium oxide (LLTO); the second ceramic powder includes at least one of aluminum oxide (Al2O3), zirconium oxide (ZrO2), and silicon oxide (SiO2). The above-mentioned ceramic powder, on the one hand, can form a mixed conductor with an organic matrix, and utilize the ionic conductivity of ceramics and the electronic insulation of organic materials to achieve ion transmission of solid electrolytes, thereby improving the ionic conductivity of solid electrolytes. On the other hand, it can also be used as rigid particles, dispersed in the organic matrix of the solid electrolyte, and can be used as a reinforcement to improve the mechanical properties of the solid electrolyte.
[0061] According to some specific embodiments of the present invention, the average particle size Dv50 of the first ceramic powder is 50nm-1000nm. For example, it can be 50nm, 100nm, 300nm, 500nm, 800nm, 1000nm, etc. The particle size of the first ceramic powder determines the film-forming performance of the electrode surface. If the particle size of the first ceramic powder is too large, the electrolyte will not be able to form a film. If the particle size of the first ceramic powder is too small, the mechanical properties of the electrolyte will be poor. As a result, it is beneficial to improve the ionic conductivity of the solid electrolyte and at the same time improve the cycle stability of the solid-state battery.
[0062] According to some specific embodiments of the present invention, the average particle size Dv50 of the second ceramic powder is 0.1 μm-1 μm. For example, it can be 0.1 μm, 0.3 μm, 0.5 μm, 0.8 μm, 1 μm, etc. The particle size of the second ceramic powder determines the film-forming performance of the electrolyte. If the particle size of the second ceramic powder is too large, the electrolyte will not be able to form a film. If the particle size of the second ceramic powder is too small, the mechanical properties of the electrolyte will be poor. As a result, it is beneficial to improve the cycle stability of the solid-state battery.
[0063] In the second aspect of the present invention, the present invention proposes a solid electrolyte. According to an embodiment of the present invention, the solid electrolyte is prepared by the above method. Based on the functional potential of polymers containing polyethylene glycol segments (such as polyethylene glycol dimethyl ether) in the field of lithium battery electrolyte / electrolyte, the present invention adopts a thermal crosslinking process, and then under the action of a nitrogen-containing crosslinking agent, the polymer containing polyethylene glycol segments and the lithium salt system are confined and solidified, and further compounded with an oxide inorganic phase powder to obtain a solid electrolyte with excellent room temperature ionic conductivity and electrochemical stability.
[0064] Furthermore, the polymer containing the polyethylene glycol segment is mixed with the first lithium salt and the nitrogen-containing crosslinking agent for heat curing, wherein the ether oxygen group in the polyethylene glycol segment can serve as a hydrogen bond acceptor, and the nitrogen-containing crosslinking agent can serve as a hydrogen bond donor, so that hydrogen bonds can be formed between the polyethylene glycol segment and the nitrogen-containing crosslinking agent, thereby achieving physical crosslinking between polymer chains and forming a three-dimensional network structure. The lithium ions decomposed from the first lithium salt can form coordination bonds with the oxygen atoms in the polyethylene glycol segment and be fixed in the three-dimensional network structure to achieve ion conduction, thereby facilitating the improvement of the ionic conductivity of the solid electrolyte, and its room temperature conductivity can reach 1×10 -4 S cm -1 Above all, the good performance foundation of the solid matrix provides convenient conditions for the selection of inorganic phase.
[0065] Furthermore, through chemical structure design and optimization of lithium salt component selection, stable, high discharge specific capacity cycle performance and rate performance with a cutoff voltage of up to 4.6V at 30°C and 0.5C can be achieved in lithium metal batteries with LiCoO2 as the positive electrode.
[0066] Furthermore, the overall solid electrolyte design and process of the present application are simple, cost-controllable, and suitable for large-scale promotion. Therefore, it has great potential application value in the development of high energy density solid-state batteries.
[0067] In the third aspect of the present invention, the present invention provides a solid electrolyte membrane. According to an embodiment of the present invention, the solid electrolyte membrane includes the solid electrolyte of the second aspect. The solid electrolyte membrane has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the solid-state battery.
[0068] According to some specific embodiments of the present invention, the method for preparing the solid electrolyte membrane comprises: placing a solid electrolyte between two layers of release films, hot pressing, and obtaining a solid electrolyte membrane. In this step, by placing the solid electrolyte between two layers of release films for pressing, the use of the release film can prevent the electrolyte material from directly contacting the mold during the pressing process, reduce the wear of the mold, and ensure that the surface of the electrolyte membrane is flat and clean. Thus, a solid electrolyte membrane with uniform thickness is obtained.
[0069] As an example, the release film includes a polytetrafluoroethylene (PTFE) film.
[0070] According to some specific embodiments of the present invention, the temperature of the hot pressing is 25°C to 80°C. For example, it can be 25°C, 30°C, 40°C, 60°C, 80°C, etc. By limiting the temperature of the hot pressing to the above range, the solid electrolyte material is helped to flow and fill better, and the interface bonding between the solid electrolyte material and the release film is promoted, which is conducive to obtaining a solid electrolyte membrane with uniform thickness.
[0071] According to the embodiments of the present application, the present application uses a polymer containing polyethylene glycol segments cured by a thermal crosslinking process as an organic matrix, uses a variety of lithium salts as lithium sources, and uses dry vibration ball milling or high-speed homogenization processes without any additional solvents to mix with Li of various oxide systems. + Conductor or non-Li + Conductive oxide ceramic powders are initially mixed. Then through grinding, rolling, cutting and other processing techniques, a self-supporting solid electrolyte membrane with high composite uniformity and good electrochemical performance is finally prepared. During the experiment, by adjusting and optimizing various parameters such as the curing process, lithium salt components, and the type and proportion of ceramic powders, the solid electrolyte material is rapidly prepared while having excellent ionic conductivity, electrode interface performance and electrochemical stability. It can be adapted to solid-state lithium batteries with high-voltage positive electrodes and lithium metal negative electrodes, and exhibits good discharge capacity and long cycle stability at room temperature, without any further optimization of the electrode itself and the interface in advance, and has great practical value.
[0072] In a fourth aspect of the present invention, the present invention provides a battery. According to an embodiment of the present application, the battery comprises the solid electrolyte membrane of the third aspect, the solid electrolyte membrane has high ionic conductivity and can modify the electrode interface, which is beneficial to improving the cycle stability of the battery.
[0073] The scheme of the present disclosure will be explained below in conjunction with the examples. It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present disclosure and should not be considered as limiting the scope of the present disclosure. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used that do not indicate the manufacturer are all conventional products that can be obtained commercially.
[0074] Example 1
[0075] 1. Preparation of solid electrolyte:
[0076] 1) In 2g of PEGDME polymer (M n =250) was added with 1.305g of LiTFSI first lithium salt (PEGDME was pre-molecularly sieved to remove water, and the lithium salt was pre-dried to remove water) and 0.2g of MBAM cross-linking agent, heated to 40°C, and magnetically stirred at 700rpm for 30min to completely dissolve the LiTFSI first lithium salt and MBAM cross-linking agent to obtain a transparent, clear solution. Then the temperature was raised to 90°C and magnetically stirred at 500rpm for 1h until the solution solidified into a semi-solid, non-fluid waxy structure. The obtained semi-solidified mixture was then transferred to a glove box filled with argon atmosphere and naturally cooled to room temperature to obtain a waxy organic matrix.
[0077] 2) 1.5 g of the organic matrix was placed in a mixing tank, 0.11 g of LiDFOB second lithium salt and 3.5 g of LTPO ceramic powder (prepared by solid phase sintering method and fully refined by planetary ball milling at 350 rpm for 24 h) were added and sealed, and then the sealed mixing tank was mixed in a Thinky MZ-8 high-speed mixer for 15 min to obtain a slurry-like solid electrolyte block, in which the mass of the LTPO ceramic powder accounted for 70% of the total mass of the organic matrix and the LTPO ceramic powder.
[0078] 2. Preparation of solid electrolyte membrane: The solid electrolyte block was transferred to a glove box, and repeatedly ground and rolled in an agate mortar for 30 minutes. Then two layers of opposite PTFE films (each with a thickness of 50 μm) were used as release films, and the solid electrolyte block was sandwiched between the two release films. The temperature of the flat hot press was set to 70°C, and the block solid electrolyte was pressed into a film. The pressure was set to 10 MPa and the pressure holding time was 3 minutes to obtain a solid electrolyte membrane.
[0079] 3. Preparation of the battery: In the battery with LiCoO2 as the positive electrode (i.e., LCO positive electrode) and lithium metal as the negative electrode, the active material ratio of the LiCoO2 positive electrode used in the test is 80wt.%, and the remaining components are 10wt.% carbon-based conductive agent and 10wt.% polyvinylidene fluoride binder. The active material surface load is about 2mg·cm -2 .
[0080] Example 2
[0081] 1. Preparation of solid electrolyte:
[0082] 1) In 2g of PEGDME polymer (M n =500) was added with 1.305g of LiTFSI first lithium salt (PEGDME was pre-molecularly sieved to remove water, and the lithium salt was pre-dried to remove water) and 0.1g of MBAM cross-linking agent, heated to 40°C, and magnetically stirred at 700rpm for 30min to completely dissolve the LiTFSI first lithium salt and MBAM cross-linking agent to obtain a transparent, clear solution. Subsequently, the temperature was raised to 90°C and magnetically stirred at 500rpm for 40min until the solution solidified into a semi-solid, non-fluid wax block structure. The obtained semi-solidified mixture was then transferred to a glove box filled with argon atmosphere and naturally cooled to room temperature to obtain a waxy organic matrix.
[0083] 2) 1.5 g of the organic matrix was placed in a mixing tank, 0.11 g of the second lithium salt of LiDFOB and 3.5 g of LTPO ceramic powder (prepared by solid phase sintering and fully refined by planetary ball milling at 350 rpm for 24 h) were added and sealed, and then the sealed mixing tank was mixed in a Thinky MZ-8 high-speed mixer for 15 min to obtain a slurry-like solid electrolyte block, in which the mass of the LTPO ceramic powder accounted for 70% of the total mass of the organic matrix and the LTPO ceramic powder.
[0084] 2. The preparation method of the solid electrolyte membrane is the same as that in Example 1.
[0085] 3. The preparation method of the battery is the same as that of Example 1.
[0086] Example 3
[0087] 1. Preparation of solid electrolyte:
[0088] 1) In 2g of PEGDME polymer (M n =250) was added with 1.305 g of LiTFSI first lithium salt (PEGDME was pre-molecularly sieved to remove water, and the lithium salt was pre-dried to remove water) and 0.2 g of MBAM cross-linking agent, heated to 40 ° C, and magnetically stirred at 700 rpm for 30 min to completely dissolve the LiTFSI first lithium salt and MBAM cross-linking agent to obtain a transparent, clear solution. Then the temperature was raised to 90 ° C, and magnetically stirred at 500 rpm for 40 min until the solution solidified into a semi-solid, non-fluid waxy structure. The obtained semi-solidified mixture was then transferred to a glove box filled with argon atmosphere and naturally cooled to room temperature to obtain a waxy organic matrix.
[0089] 2) 1.75 g of the organic matrix was placed in a mixing tank, 0.131 g of the second lithium salt of LiDFOB and 3.25 g of LLZTO ceramic powder (prepared by solid phase sintering and fully refined by planetary ball milling at 350 rpm for 24 h) were added and sealed, and then the sealed mixing tank was mixed in a Thinky MZ-8 high-speed mixer for 15 min to obtain a slurry-like solid electrolyte block, in which the mass of the LLZTO ceramic powder accounted for 65% of the total mass of the organic matrix and the LLZTO ceramic powder.
[0090] 2. The preparation method of the solid electrolyte membrane is the same as that in Example 1.
[0091] 3. Preparation of the battery: In the battery with LiFePO4 as the positive electrode and lithium metal as the negative electrode, the lithium metal battery is installed in the CR2032 button battery model. Except for the positive electrode, negative electrode and electrolyte, no additional interface modification components are added. The packaging pressure of the button battery is set to 1.25t.
[0092] Example 4
[0093] 1. Preparation of solid electrolyte:
[0094] 1) In 2g of PEGDME polymer (M n =250) was added with 1.06 g of the first lithium salt of LiFSI (PEGDME was pre-molecularly sieved to remove water, and the lithium salt was pre-dried to remove water) and 0.2 g of MBAM cross-linker, heated to 40 ° C, and magnetically stirred at 700 rpm for 30 min to completely dissolve the first lithium salt of LiFSI and the MBAM cross-linker to obtain a transparent, clear solution. Then the temperature was raised to 90 ° C and magnetically stirred at 500 rpm for 1 hour until the solution solidified into a semi-solid, non-fluid waxy structure. The obtained semi-solidified mixture was then transferred to a glove box filled with argon atmosphere and naturally cooled to room temperature to obtain a waxy organic matrix.
[0095] 2) 1.5 g of the organic matrix was placed in a mixing tank, 0.1 g of LiDFOB second lithium salt and 3.5 g of Al2O3 ceramic powder (Da Ming, Japan) were added and sealed, and then the sealed mixing tank was mixed in a Thinky MZ-8 high-speed mixer for 15 minutes to obtain a slurry-like solid electrolyte block, in which the mass of the Al2O3 ceramic powder accounted for 70% of the total mass of the organic matrix and the Al2O3 ceramic powder.
[0096] 2. The preparation method of the solid electrolyte membrane is the same as that in Example 1.
[0097] 3. The preparation method of the battery is the same as that of Example 3.
[0098] The solid electrolytes of Examples 5-14 are prepared in the same manner as in Example 1 except for some experimental parameters.
[0099] Some experimental parameters of the solid electrolytes of Examples 1-14 are shown in Table 1.
[0100] Table 1
[0101]
[0102]
[0103] Comparative Example 1
[0104] 1. Preparation of solid electrolyte:
[0105] Polymethyl methacrylate, a polymer not containing polyethylene glycol segments, was selected to replace the PEGDME polymer in Example 1, and the rest was the same as Example 1.
[0106] 2. The preparation of the solid electrolyte membrane is the same as that in Example 1.
[0107] 3. The preparation method of the battery is the same as that of Example 1.
[0108] Comparative Example 2
[0109] 1. Preparation of solid electrolyte:
[0110] Keep the co-dissolving process of PEGDME polymer and LiTFSI first lithium salt unchanged, delete the subsequent dissolution and thermal cross-linking curing process of MBAM cross-linker in the system, and obtain a mixed solution. Then, add and mix in a mortar under the protection of inert gas according to the mass ratio of LTPO ceramic powder to mixed solution of 7:3 (gradually add the mixed solution to the LTPO ceramic powder), and continue to grind, mix and roll for more than 30 minutes, and finally obtain a semi-solid electrolyte system in a slurry form.
[0111] 2. The preparation of the solid electrolyte membrane is the same as that in Example 1.
[0112] 3. The preparation method of the battery is the same as that of Example 1.
[0113] Testing and analysis
[0114] Under the same conditions, the solid electrolytes obtained in the above Examples 1-14 and Comparative Examples 1-2 were tested for ionic conductivity, and the batteries obtained in Examples 1-14 and Comparative Examples 1-2 were tested for cycle stability. The specific test methods are as follows:
[0115] Ionic conductivity test: Electrochemical impedance spectroscopy (EIS) is used to test the electrochemical response process information inside the battery. A fixed-amplitude sinusoidal voltage with a constantly changing frequency is applied to the battery. According to the corresponding sinusoidal response current signal changes, the impedance of the battery and the internal electrochemical response mechanism can be analyzed. A series of EIS tests were performed using a Biologic SP-300 electrochemical workstation with a voltage amplitude set to 50mV. In the solid electrolyte conductivity test, the positive and negative electrodes of the battery were both Li + In this paper, stainless steel gaskets are directly used as electrodes at both ends. The voltage frequency range is 1Hz to 7MHz. The apparent impedance R can be obtained by analyzing the impedance spectrum in the high-frequency region. The conductivity σ of the electrolyte can be obtained by the following formula:
[0116]
[0117] Where D is the thickness of the electrolyte, and A is the effective contact area between the electrolyte and the single-side electrode.
[0118] Cycle stability test: Assemble lithium metal full batteries to comprehensively evaluate important indicators such as rate performance, charge and discharge capacity, coulomb efficiency, and cycle stability. This type of battery uses lithium metal as the negative electrode, and the positive electrode active material is lithium iron phosphate (LiFePO4) or lithium cobalt oxide (LiCoO2). The above symmetrical battery and lithium metal battery tests are all carried out on the Blue Power CT-2001A battery test system. No additional formation is required before the cycle test.
[0119] Figure 1 The SEM micrographs of the solid electrolyte membrane of Example 1 are shown, wherein (a) is a surface SEM photograph; and (b) is a cross-sectional SEM photograph. Figure 2 A digital photograph of the solid electrolyte membrane of Example 1 is shown. Figure 1 and Figure 2 It can be observed that the solid electrolyte prepared in Example 1 has a continuous and uniform morphology, good flexibility and certain self-supporting mechanical properties.
[0120] Figure 3 The graph of the temperature-dependent ionic conductivity of the solid electrolyte of Example 1 is shown. It can be seen from the graph that the activation energy of lithium ion migration of the solid electrolyte of Example 1 is 0.31 eV, and the room temperature ionic conductivity is 3.2×10 -4 S cm -1 .
[0121] Figure 4 The LSV test diagram of the solid electrolyte of Example 1 at room temperature is shown. From the figure, it can be seen that the oxidation potential electrochemical window of the solid electrolyte of Example 1 can reach 4.7V vs.Li + / Li.
[0122] Figure 5 The long cycle discharge specific capacity-coulombic efficiency of the battery of Example 1 at 30°C and 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.45V. It can be seen from the figure that when the voltage is 4.45V, the battery exhibits 184mAh·g -1 The high initial discharge specific capacity of the battery can maintain a stable and slow capacity decay over more than 600 cycles, and the capacity retention rate after 600 cycles can reach 85.1% (154 mAh g -1 ), and maintained a full-cycle average Coulomb efficiency of more than 99.0%.
[0123] Figure 6The figure shows the long cycle discharge specific capacity-coulomb efficiency of the battery of Example 1 at 30°C and 0.5C, and the cycle cut-off voltage range is 3.0-4.6V. It can be seen from the figure that even under the extreme test condition of 4.6V, the battery can still maintain 71% of its capacity after 200 cycles (from 206mAh·g -1 Up to 147 mAh g -1 ), and its capacity decay is generally stable and uniform, which proves the performance prospects of the electrolyte of the present application in high-voltage batteries.
[0124] Figure 7 The specific capacity-voltage change of the battery of Example 1 during the long cycle at 30°C and 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.45V. It can be seen from the figure that under the 4.45V test condition, the capacity-voltage curve of the battery also shows that its capacity decay in the same cycle interval during the long cycle is uniform and stable, especially the battery's charge and discharge voltage platform has no significant change, corresponding to the stability of the positive electrode structure inside the battery and the relatively slow increase of the battery polarization.
[0125] Figure 8 The figure shows the rate performance of the battery of Example 1 at 30°C and different cut-off voltage ranges, where (a) the cut-off voltage is 4.45V; (b) the cut-off voltage is 4.6V. It can be seen from the figure that in the room temperature rate performance test of the battery in the cut-off voltage range of 3.0-4.45V, the low coulombic efficiency at 0.2C in the initial stage is due to the interface phase construction process at the beginning of the cycle and the extension of the side reaction potential plateau under low rate conditions. After about 3 cycles, the coulombic efficiency of the battery tends to stabilize. The corresponding discharge specific capacities at 0.2C, 0.5C, 1C, 2C and 5C are 184mAh·g -1 、183mAh·g -1 、175mAh·g -1 , 159mAh·g -1 and 122mAh g -1 At a higher cut-off voltage of 4.6V, the discharge capacity reached 209mAh·g at 0.2C, 0.5C, 1C, 2C and 5C respectively. -1 、192mAh·g -1 、176mAh·g -1 、158mAh·g -1 and 124mAh·g -1 The standard discharge capacity of the battery positive electrode at 4.45V and 4.6V cut-off voltages is approximately 180mAh·g -1 and 220mAh·g -1This indicates that the electrolyte provided by the present application exhibits excellent discharge capacity at room temperature.
[0126] Fig. 9 The SEM photos of the surface morphology of the positive electrode (a) and the negative electrode (b) of the battery of Example 1 after 5 cycles at 0.2C and the corresponding EDS element distribution of the positive electrode (c) and the negative electrode (b) surface are shown. The illustration in Figure (a) is the original LCO positive electrode surface morphology. The overall comparison shows that after the initial cycle, a layer of continuous interface phase that can almost effectively cover the surface is formed at the positive electrode. Compared with the loose and porous original positive electrode structure, the formation of this new phase can promote interfacial ion exchange while better isolating and protecting the side reactions between the positive electrode and the electrolyte. Its surface EDS shows that the positive electrode surface is enriched with elements such as C, F, B, and O after the cycle, and its distribution is basically consistent with the distribution of the Co element in the positive electrode active material. Therefore, this is intuitive evidence of the formation of the CEI phase. On the negative electrode side, the lithium negative electrode after the cycle is flat and smooth, and there is no structural abnormality except for the uniformly distributed granular lithium deposition. Its surface EDS shows the enrichment of C, F, and O elements, while B is not obvious relative to the distribution of other elements. This not only indicates that a protective SEI phase is also formed on the negative electrode side, but also means that the decomposition driving force of LiDFOB is stronger on the high-voltage positive electrode side. Therefore, LiDFOB is more conducive to the formation of CEI, thereby improving the stability of the high-voltage battery.
[0127] Fig.10 The negative electrode surface XPS spectrum of the battery of Example 1 after 5 cycles at 0.2C is shown. It can be seen from the figure that the negative electrode surface element spectrum confirms the existence of a series of complex SEI components reported in relevant literature, such as the main LiF, Li2O and some other lithium salts such as lithium carbonate.
[0128] Fig.11 The XPS comparison of the LCO positive electrode surface of the battery of Example 1 before and after 5 cycles at 0.2C conditions is shown. The comparison shows that the binding energy of F1s and O1s undergoes obvious chemical shift. Considering the strong electronegativity characteristics of these two elements, this means an increase in the proportion of polar chemical bonds in the positive electrode surface (electrode interface) components. Specifically, the appearance of the Li-F peak in the F1s spectrum represents the generation of LiF. The decrease in lattice oxygen intensity and the appearance of the BO peak in the O1s spectrum can correspond to the appearance of two new peaks in the B1s spectrum, indicating the decomposition of LiDFOB at the positive electrode interface and the formation of the CEI phase. The main components of this CEI phase include LiF and Li x BO y F z And a series of complex lithium salts.
[0129] Fig.12The long cycle discharge specific capacity-coulomb efficiency of the battery of Example 2 under 0.5C conditions is shown, and the cycle cut-off voltage range is 3.0-4.6 V. It can be seen from the figure that under the extreme test condition of 4.6V, its discharge capacity decreases rapidly, indicating that its cycle life stability is extremely poor and it is difficult to meet the needs of practical applications.
[0130] Fig.13 The specific capacity-voltage change of the battery of Example 2 during the long cycle at 0.5C is shown, and the cycle cut-off voltage range is 3.0-4.6 V. From the figure, it can be seen that during the cycle, while the discharge specific capacity decreases rapidly, the polarization voltage of the battery increases rapidly, and the voltage platform is extremely unstable, indicating that the internal side reactions continue to occur and the electrochemical conditions deteriorate rapidly.
[0131] The solid electrolyte of Example 1 has a lithium ion migration activation energy of 0.31 eV and an oxidation potential electrochemical window of 4.7 V vs. Li / Li. + In a battery with LiCoO2 as the positive electrode and lithium metal as the negative electrode, the cut-off voltage range is set to 3.0-4.6V, and the discharge capacity at 30°C and 0.5C is 207mAh·g -1 The capacity retention rate after 200 cycles is 71%. The cut-off voltage range is set to 3.0V to 4.45V, and the discharge capacity at 30℃ and 0.5C is 181mAh·g -1 , the capacity retention rate after 200 cycles is 85%.
[0132] The solid electrolyte of Example 2 has a lithium ion migration activation energy of 0.47 eV.
[0133] The solid electrolyte of Example 3 has a lithium ion migration activation energy of 0.35 eV. In a battery with LiFePO4 as the positive electrode and lithium metal as the negative electrode, the cut-off voltage range is set to 2.8-3.8 V, and the discharge specific capacity at 30°C and 0.5C is 139 mAh·g -1 , the capacity retention rate after 1000 cycles is 80.6%.
[0134] The solid electrolyte of Example 4 has a lithium ion migration activation energy of 0.31 eV. In a battery with LiFePO4 as the positive electrode and lithium metal as the negative electrode, the cut-off voltage range is set to 2.8-3.8 V, and the discharge specific capacity at 30°C and 0.2C is 149 mAh·g -1 , the capacity retention rate after 100 cycles is 98.0%.
[0135] The test results are shown in Table 2.
[0136] Table 2
[0137] <![CDATA[Ionic conductivity / S·cm -1 > Capacity retention after 200 cycles / % Example 1 <![CDATA[3.2×10 -4 ]]> 71% Example 2 <![CDATA[1.6×10 -5 ]]> 52% Example 3 <![CDATA[1.5×10 -4 ]]> 60% Example 4 <![CDATA[3.5×10 -4 ]]> 69% Example 5 <![CDATA[2.7×10 -4 ]]> 68% Example 6 <![CDATA[3.8×10 -4 ]]> 70% Example 7 <![CDATA[8.6×10 -6 ]]> 54% Example 8 <![CDATA[7.2×10 -5 ]]> 61% Example 9 <![CDATA[4.4×10 -4 ]]> 70% Example 10 <![CDATA[9.0×10 -6 ]]> 57% Embodiment 11 <![CDATA[4.0×10 -4 ]]> 70% Example 12 <![CDATA[9.2×10 -5 ]]> 64% Embodiment 13 <![CDATA[4.2×10 -4 ]]> 71% Embodiment 14 <![CDATA[5.7×10 -5 ]]> 50% Comparative Example 1 / / Comparative Example 2 <![CDATA[4.0×10 -4 ]]> 36%
[0138] “ / ” means none.
[0139] Combining Table 1 and Table 2, it can be seen that compared with Comparative Examples 1-2, the conductivity of the solid electrolytes of Examples 1-14 is within a reasonable range and basically meets the use requirements under room temperature conditions. Comparative Example 1 cannot form valuable ion conductivity, mainly because the dissolution, dissociation ability and effect of the first lithium salt therein are extremely poor. The lithium metal battery assembled in Comparative Example 2 exhibits an extremely poor cycle life.
[0140] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "some implementation schemes" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0141] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a solid electrolyte, characterized in that: include: Mixing a polymer, a first lithium salt and a nitrogen-containing crosslinking agent, and heating and curing the mixture to obtain an organic matrix, wherein the polymer contains a polyethylene glycol segment; The organic matrix, the second lithium salt and the ceramic powder are mixed to obtain a solid electrolyte.
2. The preparation method according to claim 1, characterized in that: The polyethylene glycol segment in the polymer includes a repeating unit -CH2CH2O-, and the molar ratio of the repeating unit -CH2CH2O- to the lithium ion in the first lithium salt is (5-20):1; Optionally, the number average molecular weight of the polymer is 200 to 1000; Optionally, the polymer comprises at least one of polyethylene glycol and polyethylene glycol dimethyl ether; Optionally, the first lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium perchlorate.
3. The preparation method according to claim 1, characterized in that: The mass of the nitrogen-containing crosslinking agent accounts for 5% to 15% of the mass of the polymer; Optionally, the cross-linking agent comprises N,N'-methylenebisacrylamide.
4. The preparation method according to claim 1, characterized in that: The curing temperature is 80°C to 100°C; Optionally, the curing time is 30 min to 60 min.
5. The preparation method according to claim 1, characterized in that: The molar amount of the second lithium salt accounts for 20% to 40% of the molar amount of the first lithium salt; Optionally, the second lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate, and lithium tetrafluoroborate.
6. The preparation method according to claim 1, characterized in that: Based on the total mass of the organic matrix and the ceramic powder, the mass of the ceramic powder accounts for 60% to 80%; Optionally, the ceramic powder includes at least one of a first ceramic powder and a second ceramic powder, wherein the first ceramic powder includes at least one of lithium lanthanum zirconium tantalum oxide, lithium tantalum phosphate, lithium aluminum titanium phosphide and lithium lanthanum titanium oxide, and the second ceramic powder includes at least one of aluminum oxide, zirconium oxide and silicon oxide.
7. The preparation method according to claim 6, characterized in that: The average particle size Dv50 of the first ceramic powder is 50nm-1000nm; Optionally, the average particle size Dv50 of the second ceramic powder is 0.1 μm-1 μm.
8. A solid electrolyte, characterized in that The solid electrolyte is prepared by the preparation method described in any one of claims 1 to 7.
9. A solid electrolyte membrane, characterized in that: The solid electrolyte membrane includes the solid electrolyte according to claim 8.
10. A battery, characterized in that: The battery comprises the solid electrolyte membrane according to claim 9.
Citation Information
Cited By
Organic composite solid electrolyte, preparation method thereof and battery
CN119419353A
Solid electrolyte, preparation method thereof and solid battery
CN120527472A
Solid-state electrolyte, method for preparing the same, and solid-state battery
CN120527472B
Solid-state electrolyte membrane and solid-state lithium battery
TWI912208B