High-transparency silicone rubber for LED lamp strip and preparation method of high-transparency silicone rubber

By using silicone rubber raw rubber with different vinyl contents and hydroxyl silicone oil and other materials, the problems of transparency and yellowing resistance of silicone rubber lamp strip materials are solved, and high transparency and excellent mechanical properties are achieved.

CN118745288AInactive Publication Date: 2024-10-08东莞市银禧特种材料科技有限公司 +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411115067.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silicone rubber lamp strip materials have limited transparency, are prone to yellowing, and are prone to bubbles during the preparation process, making them unable to meet the needs of highly transparent applications.

Method used

Methylvinyl silicone rubber raw rubber with different vinyl contents is used, and the combination of hydroxyl silicone oil and vinylhydroxyl silicone oil with white carbon black promotes the cross-linking reaction, reduces bubble generation, and improves transparency and mechanical properties.

Benefits of technology

Significantly improves the light transmittance, yellowing resistance and mechanical properties of silicone rubber, reduces the generation of bubbles, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004993397830000121
    Figure BDA0004993397830000121
  • Figure BDA0004993397830000131
    Figure BDA0004993397830000131
Patent Text Reader

Abstract

The invention provides high-transparency silicone rubber for an LED lamp strip and a preparation method of the high-transparency silicone rubber. The high-transparency silicone rubber disclosed by the invention is prepared from the following raw materials in parts by weight: 100 parts of raw rubber of methyl vinyl silicone rubber, 6 to 12 parts of hydroxyl silicone oil, 3 to 10 parts of vinyl hydroxyl silicone oil, 6 to 12 parts of dimethyl diethoxy silane, 50 to 70 parts of white carbon black and 0.05 to 1.2 parts of a release agent, the methyl vinyl silicone rubber raw rubber comprises first methyl vinyl silicone rubber raw rubber, second methyl vinyl silicone rubber raw rubber and third methyl vinyl silicone rubber raw rubber in a weight ratio of (40-60): (30-50): (5-10), and the vinyl contents of the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber are different. The silicone rubber disclosed by the invention has the characteristics of high light transmittance, yellowing resistance and excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic silicon polymer materials, and in particular to a highly transparent silicone rubber for an LED light strip and a preparation method thereof. Background Art

[0002] LED light strips are decorative items with colorful lighting effects. Through the on and off changes of the lamp beads, various dazzling and warm effects can be created. LED light strips can not only be used for interior decoration, but also for outdoor environments, adding beauty and fun to people's lives. LED light strips are mainly composed of LED lamp beads, circuit boards, power supplies and shells. The shell plays a role in protecting the internal structure of the LED light strip. Common light strip shell materials mainly include PVC and silicone rubber. Among them, PVC shell has the advantages of high hardness and good toughness, but PVC contains halogens and cannot meet people's growing requirements for environmental protection; silicone rubber shells are widely used in LED light strips because of their environmental protection, soft material, high temperature resistance, waterproof, dustproof and other advantages. However, the transparency of existing silicone rubber light strip materials has certain limitations. It is easy to turn yellow during use and it is easy to generate bubbles during the preparation process. Therefore, the existing silicone rubber cannot meet some high-transparency application requirements.

[0003] Researchers are committed to improving the transparency and comprehensive performance of silicone materials, such as yellowing resistance and weather resistance, through material innovation and process improvement. The following three factors affect the transparency of silicone materials: 1. Insufficient filling ratio of white carbon black; 2. Too much silicone oil added leads to poor transparency; 3. Process parameters are also particularly important for the transparency of materials. However, increasing the filling ratio of white carbon black will lead to higher production costs, and too little silicone oil will lead to poor compatibility between silicone rubber and white carbon black, which will lead to structuring of silicone rubber and affect its mechanical properties. It is difficult to effectively improve the transparency and comprehensive performance of silicone rubber materials by simply adjusting the process parameters.

[0004] Therefore, there is an urgent need for a highly transparent silicone rubber for LED light strips and a preparation method thereof to address the deficiencies of the prior art. Summary of the invention

[0005] The object of the present invention is to provide a highly transparent silicone rubber for LED light strips having high light transmittance, yellowing resistance and good mechanical properties, and a preparation method thereof.

[0006] To achieve the above-mentioned purpose, the present invention provides a highly transparent silicone rubber for LED light strips on one hand. The raw materials for preparation include, by weight: 100 parts of methyl vinyl silicone rubber raw rubber, 6 to 12 parts of hydroxy silicone oil, 3 to 10 parts of vinyl hydroxy silicone oil, 6 to 12 parts of dimethyl diethoxy silane, 50 to 70 parts of white carbon black and 0.05 to 1.2 parts of release agent, wherein the methyl vinyl silicone rubber raw rubber includes a first methyl vinyl silicone rubber raw rubber, a second methyl vinyl silicone rubber raw rubber and a third methyl vinyl silicone rubber raw rubber in a weight ratio of 40 to 60:30 to 50:5 to 10, and the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber have different vinyl contents.

[0007] Compared with the prior art, the raw materials for preparing the high-transparency silicone rubber for LED light strips of the present invention include the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber with different vinyl contents. By using silicone rubber raw rubbers with different vinyl contents, and controlling the weight ratio of the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber to be 40-60:30-50:5-10, the crosslinking degree of the silicone rubber material can be improved, so that the crosslinking mode is changed from "centralized crosslinking" to "dispersed crosslinking", which can significantly reduce the generation of bubbles in the silicone rubber system, thereby improving transparency and light transmittance. At the same time, the raw materials for preparing the present invention also include hydroxy silicone oil and vinyl hydroxy silicone oil, wherein the hydroxy silicone oil can react with Si-OH on white carbon black to make it hydrophobic, which helps white carbon black to be evenly dispersed in methyl vinyl silicone rubber raw rubber and prevent the structuring of mixed silicone rubber, thereby improving its mechanical properties, and the vinyl hydroxy silicone oil can accelerate the crosslinking reaction, improve strength and heat resistance, and at the same time increase the plasticity and tensile properties of the product. Therefore, the light transmittance, yellowing resistance and mechanical properties of silicone rubber can be improved by the synergistic effect of the raw materials prepared in the present invention.

[0008] As a preferred technical solution, the methyl vinyl silicone rubber raw rubber of the present invention is vinyl-terminated methyl vinyl silicone rubber raw rubber.

[0009] As a preferred technical solution, the vinyl content of the first methyl vinyl silicone rubber raw rubber of the present invention is 0.06-0.10%. By way of example, the vinyl content of the first methyl vinyl silicone rubber raw rubber may be but is not limited to 0.06%, 0.07%, 0.08%, 0.09%, or 0.10%.

[0010] Specifically, the inventors of the present invention found in the process of invention that the first methyl vinyl silicone rubber raw rubber can guarantee the performance of the product within the molecular weight range of 600,000 to 800,000. As an example, the molecular weight of the first methyl vinyl silicone rubber raw rubber can be, but is not limited to, 600,000, 620,000, 640,000, 660,000, 680,000, 700,000, 720,000, 740,000, 760,000, 780,000, and 800,000. It is necessary to explain that the present invention has no special restrictions on the source of the first methyl vinyl silicone rubber raw rubber, and it can be purchased on the market or prepared according to conventional methods known to those skilled in the art.

[0011] As a preferred technical solution, the vinyl content of the second methyl vinyl silicone rubber raw rubber of the present invention is 0.20-0.30%. As an example, the vinyl content of the second methyl vinyl silicone rubber raw rubber can be, but is not limited to, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%.

[0012] Specifically, the inventors of the present invention found in the process of invention that the second methyl vinyl silicone rubber raw rubber can guarantee the performance of the product within the molecular weight range of 600,000 to 800,000. As an example, the molecular weight of the second methyl vinyl silicone rubber raw rubber can be, but is not limited to, 600,000, 620,000, 640,000, 660,000, 680,000, 700,000, 720,000, 740,000, 760,000, 780,000, and 800,000. It is necessary to explain that the present invention has no special restrictions on the source of the second methyl vinyl silicone rubber raw rubber, and it can be purchased on the market or prepared according to conventional methods known to those skilled in the art.

[0013] As a preferred technical solution, the vinyl content of the third methyl vinyl silicone rubber raw rubber of the present invention is 1-10%. As an example, the vinyl content of the third methyl vinyl silicone rubber raw rubber can be, but is not limited to, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10%.

[0014] Specifically, the inventors of the present invention found in the process of invention that the third methyl vinyl silicone rubber raw rubber can guarantee the performance of the product within the molecular weight range of 600,000 to 800,000. As an example, the molecular weight of the second methyl vinyl silicone rubber raw rubber can be, but not limited to, 600,000, 620,000, 640,000, 660,000, 680,000, 700,000, 720,000, 740,000, 760,000, 780,000, and 800,000. It is necessary to explain that the present invention has no special restrictions on the source of the third methyl vinyl silicone rubber raw rubber, which can be purchased on the market or prepared according to conventional methods known to those skilled in the art.

[0015] As a preferred technical solution, the white carbon black of the present invention is fumed white carbon black, and the specific surface area of ​​the white carbon black is 200 to 380 m 2 / g. Specifically, the specific surface area of ​​white carbon black can be, but is not limited to, 200, 220 m 2 / g, 240m 2 / g, 260m 2 / g, 280m 2 / g、300m 2 / g, 320m 2 / g, 340m 2 / g, 360m 2 / g、380m 2 / g.

[0016] As a preferred technical solution, the hydroxyl mass content of the hydroxyl silicone oil of the present invention is 3-11%, and the viscosity is 20-50mpa.s. Specifically, the hydroxyl mass content of the hydroxyl silicone oil may be, but not limited to, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, and the viscosity may be, but not limited to, 20mpa.s, 22mpa.s, 24mpa.s, 26mpa.s, 28mpa.s, 30mpa.s, 32mpa.s, 34mpa.s, 36mpa.s, 38mpa.s, 40mpa.s, 42mpa.s, 44mpa.s, 46mpa.s, 48mpa.s, 50mpa.s.

[0017] As a preferred technical solution, the vinyl mass content of the vinyl hydroxy silicone oil of the present invention is 5-9%, the mass content of the hydroxyl group is 3-7%, and the viscosity is 30-40mpa.s. Specifically, the vinyl mass content of the vinyl hydroxy silicone oil may be, but not limited to, 5%, 6%, 7%, 8%, 9%, the mass content of the hydroxyl group may be, but not limited to, 3%, 4%, 5%, 6%, 7%, and the viscosity may be, but not limited to, 30mpa.s, 31mpa.s, 32mpa.s, 33mpa.s, 34mpa.s, 35mpa.s, 36mpa.s, 37mpa.s, 38mpa.s, 39mpa.s, 40mpa.s.

[0018] As a preferred technical solution, the release agent of the present invention is selected from at least one of stearic acid, zinc stearate, calcium stearate, magnesium stearate and aluminum stearate.

[0019] Another aspect of the present invention provides a method for preparing the highly transparent silicone rubber for the LED light strip, comprising:

[0020] (1) adding the required weight proportions of methyl vinyl silicone rubber, hydroxy silicone oil, vinyl hydroxy silicone oil, dimethyl diethoxy silane and a release agent into an internal mixer and mixing them evenly, and then adding white carbon black into the internal mixer in batches and continuing to mix them to obtain a mixed material, which is placed at room temperature;

[0021] (2) The mixed material is put into a kneader, heated and kneaded in a vacuum, and cooled and discharged.

[0022] As a preferred technical solution, in step (1), the white carbon black of the present invention can be added into the internal mixer in 9 times, and the amount added each time can be 20%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%; the time for placing at room temperature of the present invention is 6 to 24 hours, specifically, the time for placing at room temperature of the present invention can be but not limited to 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours.

[0023] As a preferred technical solution, in step (2), the vacuum degree of kneading in the present invention is 0.05-0.08 MPa, and the kneading temperature is 150-200°C. Specifically, the vacuum degree of kneading in the present invention may be but is not limited to 0.05 MPa, 0.06 MPa, 0.07 MPa, 0.08 MPa, and the kneading temperature may be but is not limited to 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 190°C, 200°C.

[0024] The present invention firstly uses an internal mixer to mix the raw materials. After mixing evenly, the raw materials are placed at room temperature for a certain period of time. Such operation can fully promote the uniform dispersion of the raw materials in the silicone rubber system of the present invention and improve the transparency and plasticity of the rubber. The mixed materials are then kneaded under the condition of a vacuum degree of 0.05-0.08MPa, and the kneading temperature is set at 150-200°C. Under this condition, low-boiling substances and water in the silicone rubber system of the present invention can be removed, so that no bubbles are generated in the subsequent extrusion process of the material, and the yellowing resistance of the highly transparent silicone rubber of the present invention can be improved. DETAILED DESCRIPTION

[0025] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0026] The raw materials used in the present invention are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0027] Example 1

[0028] The present embodiment provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.06% and the molecular weight is 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.20% and the molecular weight is 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 4% and the molecular weight is 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (the hydroxyl mass content is 5% and the viscosity is 25mPa.s), 5.1 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 6%, the hydroxyl mass content is 5% and the viscosity is 30mPa.s), 9.3 parts of dimethyl diethoxy silane, 65 parts of white carbon black (the specific surface area is 350m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0029] The method for preparing the highly transparent silicone rubber for the LED light strip of this embodiment includes:

[0030] (1) Adding the required weight proportions of methyl vinyl silicone rubber, hydroxy silicone oil, vinyl hydroxy silicone oil, dimethyldiethoxysilane and a release agent into an internal mixer and mixing them evenly, then adding white carbon black into the internal mixer for 9 times and continuing to mix, with the amount added each time being 20%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, to obtain a mixed material, which is placed at room temperature for 12 hours;

[0031] (2) The mixed material is placed in a kneader and kneaded under the conditions of a vacuum degree of 0.05 to 0.08 MPa and a kneading temperature of 160°C. After cooling to 80°C, the material is extruded.

[0032] Example 2

[0033] The present embodiment provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 44 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.06% and the molecular weight is 600,000 to 700,000), 50 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.20% and the molecular weight is 600,000 to 700,000), 6 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 4% and the molecular weight is 600,000 to 700,000), 6.5 parts of hydroxyl silicone oil (the hydroxyl mass content is 5% and the viscosity is 25mPa.s), 3.2 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 6%, the hydroxyl mass content is 5% and the viscosity is 30mPa.s), 6.2 parts of dimethyl diethoxy silane, 54 parts of white carbon black (the specific surface area is 350m 2 / g of fumed silica) and 0.06 parts of magnesium stearate.

[0034] The specific preparation method of this embodiment can refer to Example 1.

[0035] Example 3

[0036] The present embodiment provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 58 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.06% and the molecular weight is 600,000 to 700,000), 38 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.20% and the molecular weight is 600,000 to 700,000), 4 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 4% and the molecular weight is 600,000 to 700,000), 11.8 parts of hydroxyl silicone oil (the hydroxyl mass content is 5% and the viscosity is 25mPa.s), 8.6 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 6%, the hydroxyl mass content is 5% and the viscosity is 30mPa.s), 11.5 parts of dimethyl diethoxy silane, 60 parts of white carbon black (the specific surface area is 350m 2 / g of fumed silica) and 0.05 parts of magnesium stearate.

[0037] The specific preparation method of this embodiment can refer to Example 1.

[0038] Example 4

[0039] The present embodiment provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.08% and the molecular weight is 650,000 to 760,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.25% and the molecular weight is 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 6% and the molecular weight is 620,000 to 750,000), 9.3 parts of hydroxyl silicone oil (the hydroxyl mass content is 8% and the viscosity is 30 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 8%, the hydroxyl mass content is 6% and the viscosity is 25 MPa.s), 9.3 parts of dimethyl diethoxy silane, 65 parts of white carbon black (the specific surface area is 280 m 2 / g of fumed silica) and 0.12 parts of calcium stearate.

[0040] The specific preparation method of this embodiment can refer to Example 1.

[0041] Example 5

[0042] The present embodiment provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.1% and the molecular weight is 700,000 to 800,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.28% and the molecular weight is 720,000 to 780,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 8% and the molecular weight is 620,000 to 650,000), 9.3 parts of hydroxyl silicone oil (the hydroxyl mass content is 10% and the viscosity is 40mPa.s), 5.1 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 7%, the hydroxyl mass content is 4% and the viscosity is 35mPa.s), 9.3 parts of dimethyl diethoxy silane, 65 parts of white carbon black (the specific surface area is 320m 2 / g of fumed silica) and 0.12 parts of zinc stearate.

[0043] The specific preparation method of this embodiment can refer to Example 1.

[0044] Comparative Example 1

[0045] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 41 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.20% and the molecular weight is 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 4% and the molecular weight is 600,000 to 700,000), 9.3 parts of hydroxy silicone oil (the hydroxy mass content is 5% and the viscosity is 25 MPa.s), 5.1 parts of vinyl hydroxy silicone oil (the vinyl mass content is 6%, the hydroxy mass content is 5% and the viscosity is 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (the specific surface area is 350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0046] The specific preparation method of this comparative example can refer to Example 1.

[0047] Comparative Example 2

[0048] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.06% and the molecular weight is 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (the vinyl mass content is 4% and the molecular weight is 600,000 to 700,000), 6.5 parts of hydroxy silicone oil (the hydroxy mass content is 5% and the viscosity is 25mPa.s), 3.2 parts of vinyl hydroxy silicone oil (the vinyl mass content is 6%, the hydroxy mass content is 5% and the viscosity is 30mPa.s), 9.3 parts of dimethyl diethoxy silane, 54 parts of white carbon black (the specific surface area is 350m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0049] The specific preparation method of this comparative example can refer to Example 1.

[0050] Comparative Example 3

[0051] The present comparative example provides a highly transparent silicone rubber for LED light strips. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.06% and the molecular weight is 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (the vinyl mass content is 0.20% and the molecular weight is 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (the hydroxyl mass content is 5% and the viscosity is 25mPa.s), 5.1 parts of vinyl hydroxyl silicone oil (the vinyl mass content is 6%, the hydroxyl mass content is 5% and the viscosity is 30mPa.s), 65 parts of white carbon black (the specific surface area is 350m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0052] The specific preparation method of this comparative example can refer to Example 1.

[0053] Comparative Example 4

[0054] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 5.1 parts of vinyl hydroxy silicone oil (with a vinyl content of 6%, a hydroxyl content of 5%, and a viscosity of 30 mPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0055] The specific preparation method of this comparative example can refer to Example 1.

[0056] Comparative Example 5

[0057] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 mPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0058] The specific preparation method of this comparative example can refer to Example 1.

[0059] Comparative Example 6

[0060] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 40 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0061] The specific preparation method of this comparative example can refer to Example 1.

[0062] Comparative Example 7

[0063] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 mPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 mPa.s), 9.3 parts of dimethyl diethoxy silane, and 72 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0064] The specific preparation method of this comparative example can refer to Example 1.

[0065] Comparative Example 8

[0066] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 30 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 55 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 15 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0067] The specific preparation method of this comparative example can refer to Example 1.

[0068] Comparative Example 9

[0069] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 65 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 24 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 11 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0070] The specific preparation method of this comparative example can refer to Example 1.

[0071] Comparative Example 10

[0072] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0073] The preparation method of the highly transparent silicone rubber for the LED light strip of this comparative example comprises:

[0074] (1) adding required weight portions of methyl vinyl silicone rubber, hydroxy silicone oil, vinyl hydroxy silicone oil, dimethyl diethoxy silane and a release agent into an internal mixer and mixing them evenly, and then adding white carbon black into the internal mixer for 9 times and continuing to mix, with the amount added each time being 20%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, to obtain a mixed material;

[0075] (2) The above-mentioned mixed material is put into a kneader, kneaded under the conditions of a vacuum degree of 0.05 to 0.08 MPa and a kneading temperature of 160°C, cooled to 80°C and then extruded.

[0076] Comparative Example 11

[0077] The present comparative example provides a highly transparent silicone rubber for an LED light strip. The raw materials for preparation include, by weight: 51 parts of a first methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.06% and a molecular weight of 600,000 to 700,000), 41 parts of a second methyl vinyl silicone rubber raw rubber (with a vinyl content of 0.20% and a molecular weight of 600,000 to 700,000), 8 parts of a third methyl vinyl silicone rubber raw rubber (with a vinyl content of 4% and a molecular weight of 600,000 to 700,000), 9.3 parts of hydroxyl silicone oil (with a hydroxyl content of 5% and a viscosity of 25 MPa.s), 5.1 parts of vinyl hydroxyl silicone oil (with a vinyl content of 6%, a hydroxyl content of 5% and a viscosity of 30 MPa.s), 9.3 parts of dimethyl diethoxy silane, and 65 parts of white carbon black (with a specific surface area of ​​350 m 2 / g of fumed silica) and 0.12 parts of magnesium stearate.

[0078] The preparation method of the highly transparent silicone rubber for the LED light strip of this comparative example comprises:

[0079] (1) Adding the required weight proportions of methyl vinyl silicone rubber, hydroxy silicone oil, vinyl hydroxy silicone oil, dimethyldiethoxysilane and a release agent into an internal mixer and mixing them evenly, then adding white carbon black into the internal mixer for 9 times and continuing to mix, with the amount added each time being 20%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, 10%, to obtain a mixed material, which is placed at room temperature for 12 hours;

[0080] (2) The kneaded material is placed in a kneader and kneaded at a kneading temperature of 100°C. After cooling to 80°C, the mixture is extruded.

[0081] The hardness, tensile strength, elongation at break, tear strength, light transmittance and yellowing resistance of the highly transparent silicone rubber in Examples 1 to 5 and Comparative Examples 1 to 11 were tested, and the testing method is as follows.

[0082] Hardness: The hardness of the sample is measured according to the method in GB / T531.1-2008 "Test method for indentation hardness of vulcanized rubber or thermoplastic rubber - Shore durometer method";

[0083] Tensile strength: The tensile strength of the sample is measured according to the method in GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber";

[0084] Elongation at break: Determine the elongation at break of the sample according to the method in GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber";

[0085] Tear strength: The tear strength of the sample is measured according to the method in GB / T 529-2009 "Determination of tear strength of vulcanized rubber or thermoplastic rubber";

[0086] Plasticity: Determine the plasticity of the sample according to the method in GB / T 12828-2006 "Determination of plasticity and recovery value of raw rubber and unvulcanized mixed rubber";

[0087] Light transmittance: The silicone rubber composite material was calendered into a sample with a thickness of 1 mm, and the light transmittance was measured at 450 nm using an ultraviolet spectrophotometer;

[0088] Yellowing resistance: The silicone rubber composite material was rolled into a sample with a thickness of 1 mm, and the haze was measured at 450 nm using an ultraviolet spectrophotometer.

[0089] The test results are shown in Table 1.

[0090] Table 1 Test results of high transparent silicone rubber properties of Examples 1 to 5 and Comparative Examples 1 to 11

[0091]

[0092]

[0093] As shown in Table 1, Examples 1 to 5 have better mechanical properties, light transmittance and yellowing resistance than Comparative Examples 1 to 11. This may be because the raw materials for the preparation of the present invention include the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber with different vinyl contents. By using silicone rubber raw rubbers with different vinyl contents, and controlling the weight ratio of the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber to be 40 to 60:30 to 50:5 to 10, the crosslinking degree of the silicone rubber material can be improved, so that the crosslinking mode is changed from "centralized crosslinking" to "dispersed crosslinking", which can significantly reduce the generation of bubbles in the silicone rubber system, thereby improving transparency and light transmittance. At the same time, the preparation raw materials of the present invention also include hydroxy silicone oil and vinyl hydroxy silicone oil, wherein the hydroxy silicone oil can react with Si-OH on silica to make it hydrophobic, which helps to evenly disperse silica in the methyl vinyl silicone rubber raw rubber and prevent the structuring of the mixed silicone rubber, thereby improving its mechanical properties. The vinyl hydroxy silicone oil can accelerate the cross-linking reaction, improve the strength and heat resistance, and at the same time increase the plasticity and tensile properties of the product.

[0094] Specifically, it can be seen from the comparison between Example 1 and Comparative Examples 1 to 3 that the lack of any one of the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber or the third methyl vinyl silicone rubber raw rubber will result in insufficient or excessive vinyl content in the material, resulting in uneven hardness in production, insufficient vulcanization and high haze.

[0095] From the comparison between Example 1 and Comparative Examples 4 to 5, it can be seen that the lack of either hydroxy silicone oil or hydroxy vinyl silicone oil will lead to insufficient material processing and insufficient crosslinking. Although the material transparency can be provided to a large extent, it is difficult to absorb powder and the operation is difficult.

[0096] From the comparison between Example 1 and Comparative Examples 6 to 7, it can be seen that when the weight percentage of white carbon black exceeds the range of the present invention, it will be difficult to absorb the powder and an effective production process cannot be formed; when the weight percentage of white carbon black is lower than the range of the present invention, the transparency of the material will be insufficient.

[0097] From the comparison between Example 1 and Comparative Examples 8 to 9, it can be seen that when the weight ratio of the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber exceeds the range recorded in this application, the hardness of the material will fluctuate greatly, and the elongation will tend to the two ends, which is not suitable for product application.

[0098] From the comparison between Example 1 and Comparative Example 10, it can be seen that if the material is not placed at room temperature after the mixing is completed, the transparency of the material will be low and the haze will be high.

[0099] From the comparison between Example 1 and Comparative Example 11, it can be seen that when kneading is not performed under vacuum conditions and the kneading temperature is lower than the temperature recorded in the present invention, the material will have low molecular weight, affecting the molding, transparency and yellowing resistance of the material.

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A highly transparent silicone rubber for LED light strip, characterized in that: The raw materials include, by weight, 100 parts of methyl vinyl silicone rubber raw rubber, 6 to 12 parts of hydroxy silicone oil, 3 to 10 parts of vinyl hydroxy silicone oil, 6 to 12 parts of dimethyl diethoxy silane, 50 to 70 parts of white carbon black and 0.05 to 1.2 parts of release agent, wherein the methyl vinyl silicone rubber raw rubber includes a first methyl vinyl silicone rubber raw rubber, a second methyl vinyl silicone rubber raw rubber and a third methyl vinyl silicone rubber raw rubber in a weight ratio of 40 to 60:30 to 50:5 to 10, and the first methyl vinyl silicone rubber raw rubber, the second methyl vinyl silicone rubber raw rubber and the third methyl vinyl silicone rubber raw rubber have different vinyl contents.

2. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The vinyl content of the first methyl vinyl silicone rubber is 0.06-0.10%.

3. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The content of vinyl in the second methyl vinyl silicone rubber is 0.20-0.30%.

4. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The content of vinyl in the third methyl vinyl silicone rubber raw rubber is 1-10%.

5. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The white carbon black is fumed white carbon black, and the specific surface area of ​​the white carbon black is 200 to 380 m 2 / g.

6. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The hydroxyl content of the hydroxy silicone oil is 3-11% by mass and the viscosity is 20-50 mPa.s.

7. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The vinyl content of the vinyl hydroxy silicone oil is 5-9% by weight, and the hydroxyl content is 3-7% by weight.

8. The highly transparent silicone rubber for LED light strip according to claim 1, characterized in that: The release agent is selected from at least one of stearic acid, zinc stearate, calcium stearate, magnesium stearate and aluminum stearate.

9. A method for preparing the highly transparent silicone rubber for LED light strip according to any one of claims 1 to 8, characterized in that: include: (1) adding the required weight proportions of methyl vinyl silicone rubber, hydroxy silicone oil, vinyl hydroxy silicone oil, dimethyl diethoxy silane and a release agent into an internal mixer and mixing them evenly, and then adding white carbon black into the internal mixer in batches and continuing to mix them to obtain a mixed material, which is placed at room temperature; (2) The mixed material is put into a kneader, heated and kneaded in a vacuum, and cooled and discharged.

10. The method for preparing highly transparent silicone rubber for LED light strip according to claim 9, characterized in that: In step (1), the standing time is 6 to 24 hours; in step (2), the kneading vacuum degree is 0.05 to 0.08 MPa, and the kneading temperature is 150 to 200°C.

Citation Information

Patent Citations

  • Full-transparent liquid silicone rubber composition and preparation method thereof

    CN102924927A

  • Low-water-absorption high-transparency precipitated silicone rubber and preparation method thereof

    CN114686001A