Method for leaching lithium, nickel, cobalt and manganese from waste LNCM type lithium ion battery positive electrode material
Through deep eutectic solvent leaching technology, the problems of harsh reaction conditions and low leaching rate in lithium-ion battery recycling are solved, and efficient recycling of lithium, nickel, cobalt, and manganese is achieved, reducing recycling costs and reducing environmental pollution.
Patent Information
- Application Number
- CN202410800232.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-08
AI Technical Summary
Existing lithium-ion battery recycling technology has problems such as harsh reaction conditions, low leaching rate, and difficult and toxic solvents to degrade, resulting in environmental pollution and high economic costs.
Ascorbic acid and thiatin dimethyl-β-propionate are used to configure a deep eutectic solvent. The lithium, nickel, cobalt and manganese in the waste LNCM lithium-ion battery cathode material is leached through the deep eutectic solvent, and the leaching time is shortened to 14 minutes. Lithium, The leaching efficiency of nickel, cobalt and manganese reaches more than 99%, avoiding toxic solvents and high temperature treatment.
It realizes low-cost, fast and efficient recycling of lithium-ion battery cathode materials, reduces the recycling cost of used ternary lithium batteries, and reduces the harm to the environment.
Abstract
Description
Technical Field
[0001] The invention relates to a method for leaching lithium, nickel, cobalt and manganese from anode materials of waste LNCM lithium ion batteries, belonging to the technical field of recycling waste lithium batteries. Background Art
[0002] Lithium-ion batteries (LIBs) fail due to irreversible changes in their internal structure after countless charge and discharge cycles. The cathode materials of failed LIBs contain precious metal ions such as Co, Ni, Mn and Li, and the metal ions in these cathode materials can cause soil and water pollution, leading to environmental problems and ecological degradation.
[0003] Currently, lithium-ion battery recycling can be divided into three categories: pyrometallurgy, hydrometallurgy, and direct recycling. Pyrometallurgy is the most commonly used method, which can achieve a 100% recovery rate by melting battery materials at high temperatures; however, this method produces harmful pollutants that are detrimental to the environment and requires more steps, and the recovered valuable metals cannot be used directly in electrode manufacturing. Hydrometallurgy can be more flexible in extraction and purification after chemical solvents have leached the target metal, but there is a problem of difficulty in separation when separating similar elements, and it will produce a lot of waste and pose risks to the environment.
[0004] Therefore, existing pyrometallurgy and hydrometallurgy have problems in terms of economy and sustainability. Direct recycling is more attractive by retaining the cathode crystal structure to directly regenerate battery components, reduce energy consumption and waste. However, this technology has not been widely adopted due to its poor development due to input chemical sensitivity and poor quality of recycled battery materials. Therefore, appropriate methods are needed to sustainably recycle lithium-ion batteries and a green, efficient and gentle system is urgently needed. Summary of the invention
[0005] In view of the problems of harsh reaction conditions, low leaching rate, difficult to degrade and toxic solvents in the current leaching process of lithium ion battery positive electrode materials, the present invention proposes a method for leaching lithium, nickel, cobalt and manganese from waste LNCM lithium ion battery positive electrode materials, and uses ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor to configure a deep eutectic solvent. The deep eutectic solvent is used to leach lithium, nickel, cobalt and manganese in waste LNCM lithium ion battery positive electrode materials, and the leaching time can be shortened to less than 14 minutes, and the leaching efficiency of lithium, nickel, cobalt and manganese is more than 99%. The process flow of the present invention has the characteristics of low cost, fast and high efficiency, and can effectively reduce the recovery cost of waste ternary lithium battery positive electrode materials.
[0006] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0007] (1) using ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, mixing ascorbic acid and dimethyl-β-thiophene propionate uniformly and dissolving them in deionized water at a temperature of 40 to 80° C., and cooling to room temperature to obtain a deep eutectic solvent;
[0008] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, and the waste battery positive electrode powder is added to a deep eutectic solvent and leached at a temperature of 40 to 70° C. for 3 to 15 minutes to obtain a lithium nickel cobalt manganese leaching solution.
[0009] In the step (1), the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 4:1 to 1:4.
[0010] The mass content of deionized water in the deep eutectic solvent in step (1) is 30-85%.
[0011] In the step (2), the solid-to-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 10 to 40:1.
[0012] The calculation formula for the leaching rate of Ni, Co, Mn and Li in the positive electrode material of waste LNCM lithium-ion batteries is as follows:
[0013] η=[(C Me ×V) / (w Me ×m)]×100%, where C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material.
[0014] The present invention adopts the principle of leaching Ni, Co, Mn and Li in the cathode material of waste LNCM lithium-ion batteries by deep eutectic solvent:
[0015] (1) The hydrogen ions ionized from ascorbic acid in the deep eutectic solvent combine with the oxygen in the metal oxygen bond in the cathode material to generate water, which destroys the layered structure of the cathode material and promotes the release of metal ions; (2) Ni in the cathode material 3+ 、Co 3+ , Mn 4+ High-valent metal ions are reduced to Ni 2+ 、Co 2+ , Mn 2+Low-valent metal ions; (3) The reduced low-valent metal ions form complexes with the chloride ions in dimethyl-β-thiophene propionate. Due to the presence of water, part of the chloride complex is hydrolyzed to form a complex of hydrated metal ions, and finally the complex of chlorinated metal ions and the complex of hydrated metal ions reach coordination equilibrium.
[0016] The beneficial effects of the present invention are:
[0017] (1) The present invention uses ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor to configure a deep eutectic solvent, and uses the deep eutectic solvent to leach lithium, nickel, cobalt and manganese in the cathode material of waste LNCM lithium-ion batteries, which can shorten the leaching time to less than 14 minutes, and the leaching efficiency of lithium, nickel, cobalt and manganese is more than 99%;
[0018] (2) The present invention uses a deep eutectic solvent to leach lithium, nickel, cobalt and manganese from the positive electrode material of waste LNCM lithium-ion batteries, avoiding the use of toxic solvents, strong acids, strong bases and reducing agents, and makes ascorbic acid and dimethyl-β-thiophene propionate naturally degradable, thereby reducing the harm to the environment;
[0019] (3) The process of the present invention has the advantages of simple operation, low reaction temperature, short leaching time and extremely high leaching efficiency during the entire leaching process. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0021] Example 1: In terms of mass percentage, the waste NCM111 lithium-ion battery positive electrode material in this example contains 6.5% Li, 20.9% Ni, 20.4% Co and 18.2% Mn;
[0022] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0023] (1) using ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, mixing ascorbic acid and dimethyl-β-thiophene propionate uniformly and dissolving them in deionized water at a temperature of 40° C. and stirring (600 rpm), and cooling to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 4:1, and the mass content of deionized water in the deep eutectic solvent is 30%;
[0024] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 40° C. for 15 minutes to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 10:1;
[0025] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0026] η=[(C Me ×V) / (w Me ×m)]×100%
[0027] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0028] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 95.70%, 97.15%, 98.51% and 99.61% respectively.
[0029] Example 2: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0030] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0031] (1) With ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, ascorbic acid and dimethyl-β-thiophene propionate are mixed uniformly and dissolved in deionized water at a temperature of 50° C. and stirred (650 rpm), and then cooled to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 3:1, and the mass content of deionized water in the deep eutectic solvent is 40%;
[0032] (2) The waste NCM111 lithium-ion battery positive electrode material is crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 50° C. for 12 minutes to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 15:1;
[0033] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0034] η=[(C Me ×V) / (w Me ×m)]×100%
[0035] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0036] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 96.50%, 98.05%, 98.58% and 99.71% respectively.
[0037] Example 3: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0038] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0039] (1) With ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, ascorbic acid and dimethyl-β-thiophene propionate are mixed uniformly and dissolved in deionized water at 60° C. and cooled to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 2:1, and the mass content of deionized water in the deep eutectic solvent is 65%;
[0040] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 60° C. for 9 minutes to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 25:1;
[0041] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0042] η=[(C Me ×V) / (w Me×m)]×100%
[0043] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0044] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 98.09%, 98.44%, 98.64% and 99.77% respectively.
[0045] Example 4: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0046] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0047] (1) using ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, mixing ascorbic acid and dimethyl-β-thiophene propionate uniformly and dissolving them in deionized water at 70° C. and cooling to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 1:1, and the mass content of deionized water in the deep eutectic solvent is 70%;
[0048] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 65° C. for 5 min to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 30:1;
[0049] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0050] η=[(C Me ×V) / (w Me ×m)]×100%
[0051] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Meis the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0052] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 98.59%, 98.49%, 98.54% and 99.65% respectively.
[0053] Example 5: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0054] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0055] (1) With ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, ascorbic acid and dimethyl-β-thiophene propionate are mixed uniformly and dissolved in deionized water at 60° C. and cooled to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 1:2, and the mass content of deionized water in the deep eutectic solvent is 50%;
[0056] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 60° C. for 10 min to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 25:1;
[0057] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0058] η=[(C Me ×V) / (w Me ×m)]×100%
[0059] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0060] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 98.05%, 98.65%, 98.28% and 99.18% respectively.
[0061] Example 6: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0062] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0063] (1) With ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, ascorbic acid and dimethyl-β-thiophene propionate are mixed uniformly and dissolved in deionized water at 65° C. and cooled to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 1:3, and the mass content of deionized water in the deep eutectic solvent is 45%;
[0064] (2) The waste NCM111 type lithium-ion battery positive electrode material is crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 50° C. for 12 minutes to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 30:1;
[0065] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0066] η=[(C Me ×V / (w Me ×m)]×100%
[0067] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0068] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 98.65%, 98.72%, 98.34% and 99.41% respectively.
[0069] Example 7: The cathode material of the waste NCM111 lithium-ion battery in this example is the same as that in Example 1;
[0070] A method for leaching lithium, nickel, cobalt and manganese from waste NCM111 lithium-ion battery positive electrode materials, the specific steps are as follows:
[0071] (1) With ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, at a temperature of 80° C. and stirring (700 rpm), ascorbic acid and dimethyl-β-thiophene propionate are mixed uniformly and dissolved in deionized water, and then cooled to room temperature to obtain a deep eutectic solvent; the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 1:4, and the mass content of deionized water in the deep eutectic solvent is 85%;
[0072] (2) Waste NCM111 lithium-ion battery positive electrode materials are crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 70° C. for 3 min to obtain a lithium nickel cobalt manganese leaching solution; the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 40:1;
[0073] The contents of Ni, Co, Mn and Li in the lithium nickel cobalt manganese leaching solution were determined by inductively coupled plasma emission spectrometer, and the leaching rates of Ni, Co, Mn and Li in the positive electrode powder of waste NCM111 lithium-ion battery were calculated by the following formula:
[0074] η=[(C Me ×V) / (w Me ×m)]×100%
[0075] In the formula, C Me is the metal ion (Me=Li, Ni, C, Mn) in the leachate, concentration (mg / L), V is the volume of the leachate (L), m is the mass of the cathode active material (g); w Me is the mass fraction (wt%) of the metal in the cathode active material. After leaching is completed, the solution is filtered and there is no black residue, indicating that the valuable metal in the positive electrode material is completely leached;
[0076] The leaching rates of Ni, Co, Mn and Li were calculated by the leaching rate formula to be 98.73%, 99.30%, 99.75% and 99.04% respectively.
[0077] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for leaching lithium, nickel, cobalt and manganese from waste LNCM type lithium ion battery positive electrode materials, characterized in that: The specific steps are as follows: (1) using ascorbic acid as a hydrogen bond acceptor and dimethyl-β-thiophene propionate as a hydrogen bond donor, mixing ascorbic acid and dimethyl-β-thiophene propionate uniformly and dissolving them in deionized water at a temperature of 40 to 80° C., and cooling to room temperature to obtain a deep eutectic solvent; (2) The waste LNCM type lithium ion battery positive electrode material is crushed and sieved to obtain waste battery positive electrode powder, the waste battery positive electrode powder is added to a deep eutectic solvent, and leached at a temperature of 40 to 70° C. for 3 to 15 minutes to obtain a lithium nickel cobalt manganese leaching solution.
2. The method for leaching lithium nickel cobalt manganese from waste LNCM type lithium ion battery positive electrode materials according to claim 1, characterized in that: In step (1), the molar ratio of ascorbic acid to dimethyl-β-thiophene propionate is 4:1 to 1:
4.
3. The method for leaching lithium nickel cobalt manganese from waste LNCM type lithium ion battery positive electrode materials according to claim 1, characterized in that: The mass content of deionized water in the deep eutectic solvent of step (1) is 30-85%.
4. The method for leaching lithium nickel cobalt manganese from waste LNCM type lithium ion battery positive electrode materials according to claim 1, characterized in that: In step (2), the solid-liquid ratio g:L of the waste battery positive electrode powder and the deep eutectic solvent is 10 to 40:1.
Citation Information
Cited By
Manganese adsorbent and preparation method thereof
CN120398123A
Method for preparing single crystal ternary lithium positive electrode by recycling waste sodium battery based on deep eutectic solvent-solvent thermal regeneration system
CN120955250A
Preparation method of lithium ion battery conductive polymer binder with double solubility as well as product and application of lithium ion battery conductive polymer binder
CN121379447A
Method for recycling valuable metal from waste lithium battery
CN122081656A
Method for recycling valuable metals from waste lithium batteries
CN122081656B