Method for preparing low-impurity rare earth feed liquid by using cerium-based material
Through the redox and precipitation adsorption technology of cerium-based materials, the problem of long process and high cost of removing impurities such as aluminum in the existing rare earth metallurgical technology is solved. Low-impurity rare earth liquid is prepared, which improves the quality of rare earth products and the utilization of resources. Balanced utilization.
Patent Information
- Application Number
- CN202410714140.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-04
AI Technical Summary
In existing rare earth metallurgical technology, the process of removing impurities such as aluminum has problems such as long process, high cost and limited raw materials. It is difficult to effectively prepare low-impurity rare earth liquids, which affects the quality of rare earth products and the balanced utilization of resources.
Cerium-based materials are used to regulate the pH value through redox, precipitation and adsorption reactions, precipitate and adsorb impurities, achieve solid-liquid separation, and prepare low-impurity rare earth material liquids.
It has achieved a significant reduction in the content of impurities such as aluminum, iron, uranium, and thorium, simplified the subsequent extraction and separation process, reduced production costs, and improved product purity and resource utilization efficiency.
Smart Images

Figure CN118745532A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth metallurgy, and in particular relates to a method for preparing a low-impurity rare earth liquid by using a cerium-based material. Background Art
[0002] As an important strategic resource in my country, rare earth is one of the key materials indispensable for transforming and upgrading traditional industries, developing strategic emerging industries and national defense science and technology industries. my country is the country with the richest rare earth resources in the world. Ion adsorption type rare earth ore has become a very important strategic resource in my country because it is rich in medium and heavy rare earths. The mass percentage of impurities such as aluminum and iron in ion adsorption type rare earth ore is 0.5%-10%. In the separation production process, the concentrate is dissolved by adding hydrochloric acid to obtain rare earth liquid, and the liquid is separated by extraction to obtain a chloride solution of one or several rare earths, and finally rare earth oxides are obtained by precipitation and burning. Impurity aluminum element accounts for a high proportion in the original ore and is dissolved with rare earths during acid dissolution; dissolved aluminum is easy to be enriched in the extractant, reducing the separation and processing capacity of the extractant; further, due to the change of pH value during the extraction process, the colloidal aluminum hydroxide generated is easy to form a three-phase substance that affects the separation process. Taking the solution obtained from the acid dissolution workshop of a southern mineral separation enterprise as an example, the concentration of the dissolved rare earth solution is 1.51mol / L, of which the impurity Al2O3 is 3624mg / L, Al2O3 / REO=1.42%; other impurities: F1540mg / L, Fe2O330mg / L, U 210mg / L, Th 36mg / L, Cr 0.35mg / L. Impurities such as aluminum are enriched to varying degrees, which seriously affects the quality of rare earth products. With the development of technology, the research and development and application of high-end materials require a large amount of high-purity rare earth products.
[0003] At the same time, rare earths include 17 elements such as lanthanum, cerium, praseodymium, neodymium, terbium, dysprosium, and yttrium. The distribution and use of each element are different. The high-abundance elements lanthanum, cerium, and yttrium account for about 50% in total, but their application is limited, which makes it difficult to achieve balanced utilization of rare earth elements, affecting the value of rare earth resources. In recent years, the total supply of rare earths has gradually increased, and the total amount of domestic rare earth smelting and separation has continuously set new highs. The backlog of high-abundance rare earth products such as cerium in various rare earth groups has intensified. Therefore, it is urgent to develop technologies for removing impurities such as aluminum for industrial production to prepare low-impurity rare earth liquids and promote the balanced application of high-abundance rare earths.
[0004] At present, most production companies mainly use extraction, precipitation, and activation-dissolution methods to remove impurities such as aluminum to prepare low-impurity rare earth liquid.
[0005] In the existing separation method for removing aluminum from rare earth liquid by extraction, cyclopentane acid is used as an extractant. This process has the advantages of low production cost, good aluminum removal effect, and small loss of rare earth elements. Chinese patents CN103773955 and CN101979680 both use cyclopentane acid-alcohol-kerosene system to obtain rare earth liquid with relatively low impurity aluminum content through multi-stage saponification, extraction, washing, and stripping. The process is relatively stable. The current problems mainly include aging of the organic phase, reduced process efficiency caused by esterification reaction between cyclopentane acid and alcohol, and difficulty in phase separation caused by aluminum hydrolysis.
[0006] Precipitation aluminum removal mainly includes alkaline precipitation and acid precipitation. Chinese patent CN 110451539 uses alkaline solutions such as ammonium bicarbonate to adjust the pH value of the feed solution, and preferentially precipitates aluminum hydroxide. After solid-liquid separation, rare earth feed solution is obtained. The higher the aluminum hydroxide precipitation rate of this method, the greater the rare earth co-precipitation rate. The obtained neutralization and aluminum removal slag still needs to be treated with strong alkali and filtered multiple times, and the reaction process is relatively long. Chinese patents CN103194627 and CN116179876 use oxalic acid precipitation to precipitate rare earths. Impurities such as aluminum and iron are complexed with oxalic acid and remain in the precipitation mother liquor to achieve separation of impurities and rare earths. When there is more aluminum and iron in the oxalic acid precipitation method, the cost increases significantly.
[0007] Chinese patent CN113046578 proposes to remove aluminum from the upstream, that is, rare earth oxide concentrate, and prepare low-impurity rare earth liquid by activation-dissolution method. This process has the advantages of high efficiency, short process, and ideal removal of impurities such as aluminum. It has been promoted and applied by many rare earth separation enterprises in southern mines in my country. However, this method has a certain scope of application, and is currently mainly applicable to raw materials containing rare earth oxides. Summary of the invention
[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a low-impurity rare earth liquid using a cerium-based material. The method is efficient, short-process, low-cost, has a wide range of applications, and is suitable for large-scale industrial production. The prepared rare earth liquid has lower contents of common non-rare earth impurities such as aluminum, iron, uranium, thorium, and fluorine, especially lower impurity aluminum content; the method overcomes the problems of long process, high cost, and raw material restrictions in the existing rare earth liquid aluminum removal process.
[0009] To achieve the above purpose, the technical solution adopted by the present invention is: a method for preparing a low-impurity rare earth liquid using a cerium-based material, the method comprising the following steps:
[0010] S1. Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction;
[0011] S2. Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction;
[0012] S3, adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurity precipitation;
[0013] S4, solid-liquid separation: The low-impurity rare earth feed liquid is obtained by performing solid-liquid separation on the rare earth feed liquid and the solid that has adsorbed impurities.
[0014] Furthermore, the impure rare earth solution is a hydrochloric acid and / or nitric acid rare earth solution, and the impurities in the impure rare earth solution include one or more of aluminum, iron, fluorine, uranium, and thorium.
[0015] Furthermore, in the rare earth solution containing impurities, the concentration of rare earth elements is 0.1 to 2.5 mol / L; and the pH value of the rare earth solution containing impurities is <5.5.
[0016] Furthermore, the cerium-based material is selected from one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite material, cerium hydroxide-non-cerium rare earth composite material, cerium dioxide-non-rare earth metal composite material, cerium hydroxide-non-rare earth metal composite material, cerium dioxide-containing slag, and cerium hydroxide-containing slag.
[0017] Furthermore, the reducing agent includes one or more of citric acid, thiourea, urea, hydroxylamine hydrochloride, hydrogen peroxide, iron powder, and glucose.
[0018] Furthermore, the molar ratio of the cerium-based material to the reducing agent is 10:1 to 1:10.
[0019] Furthermore, in step S1, the temperature of the redox reaction is 10-100° C., and the reaction time is 0.5-100 h.
[0020] Further, in step S2, the pH value of the reaction system is regulated by adding a pH regulating agent;
[0021] The pH value regulating reagent includes one or more of sodium hydroxide, ammonia water, ammonium bicarbonate, sodium bicarbonate, ammonium carbonate, sodium carbonate, rare earth hydroxide, composite rare earth hydroxide, and rare earth oxide.
[0022] Further, in step S2, the pH value of the reaction system is controlled to be between 1 and 5;
[0023] The temperature of the precipitation reaction is 10-100° C., and the precipitation reaction time is 0.5-100 h.
[0024] Furthermore, in step S3, the precipitation reaction end point pH value is 2.5-5.
[0025] Furthermore, in step S3, the reaction temperature for continuing the reaction while maintaining the pH value at the end point of the precipitation reaction is 10 to 100° C., and the reaction time is 0.5 to 24 hours.
[0026] Furthermore, in step S4, the solid-liquid separation method includes natural filtration, suction filtration or pressure filtration.
[0027] The beneficial effects of the present invention are: the method for preparing a low-impurity rare earth liquid using a cerium-based material provided by the present invention can reduce the content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium in the prepared rare earth liquid, especially reduce the content of aluminum. The beneficial effects of the present invention are specifically embodied in:
[0028] (1) The rare earth liquid containing impurities is used as the treatment object, and the application range is wide;
[0029] (2) By producing impurity precipitation and efficient adsorption of common non-rare earth impurities such as aluminum, iron, uranium, thorium, and fluorine in a reaction system with a relatively low pH value, a low-impurity feed liquid is prepared, which is beneficial to the subsequent rare earth extraction and separation process, increases the organic phase extraction and separation capacity, and effectively reduces the cost of extraction and separation;
[0030] (3) The prepared low-impurity rare earth liquid has lower uranium and thorium contents, further reducing the radioactivity of the product; at the same time, the prepared low-impurity rare earth liquid has low aluminum, iron and fluorine contents, making it easier to obtain high-purity rare earth products.
[0031] The present invention starts from the rare earth liquid containing impurities and innovatively combines the variable valence characteristics of cerium element +4 / +3 and the large surface area adsorption performance of cerium oxide matching the pH value of impurity precipitation. 4+ / Ce 3+ The conversion between them is carried out, and the pH value of the reaction system is regulated with the aid of a pH regulator, so that common non-rare earth impurities are precipitated at a lower pH value; and through the partial dissolution of cerium dioxide, large specific surface area cerium is produced, and the impurity precipitation is matched for efficient adsorption, so as to achieve the removal of common non-rare earth impurities, and a low-impurity rare earth liquid is prepared by solid-liquid separation.
[0032] The method provided by the present invention can produce a rare earth liquid with a low content of common non-rare earth impurities such as aluminum, iron, uranium, and thorium, which is conducive to the rare earth separation production process and the improvement of product quality. At the same time, the method provided by the present invention is in line with the current process, the effective utilization rate of the equipment is high, and it has the characteristics of high efficiency and short process, and is suitable for large-scale industrial production. Moreover, the method provided by the present invention has a significant effect on impurity removal, and realizes the efficient separation of rare earth and impurities such as aluminum; and it can save the cost of burning mixed rare earth hydrochloride and the cost of subsequent extraction and separation processes, reduce the overall production cost of rare earth products, and increase the added value of products. It has important practical significance for giving full play to my country's rare earth resource advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic flow chart of a method for preparing a low-impurity rare earth solution using a cerium-based material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be further clearly and completely described below in conjunction with the drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] The method for preparing a low-impurity rare earth liquid using a cerium-based material provided in this embodiment starts from the rare earth liquid containing impurities and innovatively combines the +4 / +3 variable valence property of cerium element and the large surface area adsorption performance of cerium oxide matching the pH value of impurity precipitation. 4+ / Ce 3+ The conversion between them is carried out, and the pH value of the reaction system is regulated with the aid of a pH regulator, so that common non-rare earth impurities are precipitated at a lower pH value; and through the partial dissolution of cerium dioxide, a large specific surface area cerium is produced, and the impurity precipitation is matched for efficient adsorption, so as to achieve the removal of common non-rare earth impurities, and a low-impurity rare earth liquid is prepared by solid-liquid separation.
[0036] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a low-impurity rare earth liquid using a cerium-based material, the method comprising the following steps:
[0037] S1. Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction;
[0038] Specifically, the oxidation-reduction process in step S1 is to add a certain proportion of cerium-based material and reducing agent to the rare earth liquid containing impurities, and the two are mixed and reacted at a certain temperature for a period of time, and an oxidation-reduction reaction occurs between cerium dioxide in the cerium-based material and the reducing agent, and part of the cerium is dissolved; part of the cerium element in the cerium-based material is oxidized from +4 valence to +3 valence.
[0039] Optionally, the cerium-based material is selected from one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite material, cerium hydroxide-non-cerium rare earth composite material, cerium dioxide-non-rare earth metal composite material, cerium hydroxide-non-rare earth metal composite material, cerium dioxide-containing slag, and cerium hydroxide-containing slag; wherein cerium dioxide / cerium hydroxide accounts for 1% to 100%.
[0040] Optionally, the impure rare earth solution is a hydrochloric acid and / or nitric acid rare earth solution, and the impurities in the impure rare earth solution include one or more of aluminum, iron, fluorine, uranium and thorium.
[0041] Specifically, the concentration of rare earth elements in the rare earth solution containing impurities is 0.1-2.5 mol / L; the pH value of the rare earth solution containing impurities is <5.5.
[0042] Optionally, the reducing agent includes one or more of citric acid, thiourea, urea, hydroxylamine hydrochloride, hydrogen peroxide, iron powder, and glucose.
[0043] Optionally, the molar ratio of the cerium-based material to the reducing agent is 10:1 to 1:10; the molar ratio of the cerium-based material to the rare earth element in the rare earth liquid containing impurities is 1:100 to 10:1.
[0044] Specifically, the temperature of the redox reaction is 10 to 100° C., and the reaction time is 0.5 to 100 hours.
[0045] S2. Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction;
[0046] Specifically, the precipitation reaction process in step S2 is to control the pH value of the reaction system by controlling the degree of reaction between the cerium-based material and the reducing agent and adding a certain amount of pH regulating reagent. Common non-rare earth impurities such as aluminum, iron, uranium, thorium, and fluorine in the rare earth liquid are precipitated as the precipitation reaction proceeds.
[0047] Optionally, in step S2, the pH value of the reaction system is regulated by adding a certain amount of pH regulating reagent, and the pH regulating reagent includes one or more of sodium hydroxide, ammonia water, ammonium bicarbonate, sodium bicarbonate, ammonium carbonate, sodium carbonate, rare earth hydroxide, composite rare earth hydroxide, and rare earth oxide.
[0048] Specifically, in step S2, the temperature of the precipitation reaction is 10-100° C., the precipitation reaction time is 0.5-100 h, and the pH value of the reaction system is controlled between 1 and 5.
[0049] S3, adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurity precipitation;
[0050] Optionally, in the impurity adsorption process in step S3, when the pH value reaches the impurity precipitation end point, the cerium-based material forms an adsorption material with a large specific surface area due to partial dissolution of cerium dioxide, which can effectively adsorb the impurity precipitates in the liquid phase.
[0051] Optionally, in step S3, the precipitation reaction end point pH value is 2.5-5.
[0052] Specifically, in step S3, the reaction temperature for continuing the reaction while maintaining the pH value at the end point of the precipitation reaction is 10 to 100° C., and the reaction time is 0.5 to 24 hours.
[0053] S4, solid-liquid separation: preparing the low-impurity rare earth feed liquid by performing solid-liquid separation on the rare earth feed liquid and the solid that has adsorbed impurities;
[0054] Optionally, the solid-liquid separation process in step S4 is to separate the rare earth liquid and the solid that has adsorbed impurities by simple methods such as natural filtration, suction filtration or filter press to obtain the low-impurity rare earth liquid.
[0055] In a specific embodiment, the impurities in the low-impurity rare earth solution include aluminum, iron, uranium, thorium, and fluorine, wherein the aluminum content is 1 to 300 mg / L, the iron content is 1 to 300 mg / L, the uranium content is 0.01 to 10 mg / L, the thorium content is 0.01 to 10 mg / L, and the fluorine content is 1 to 300 mg / L.
[0056] The method for preparing a low-impurity rare earth liquid using a cerium-based material provided in the present embodiment can use a rare earth liquid containing impurities as a treatment object, and has a wide range of applications. A certain proportion of cerium-based materials and a reducing agent are added to the rare earth liquid containing impurities through an oxidation-reduction process, and an oxidation-reduction reaction occurs between cerium dioxide in the cerium-based material and the reducing agent to dissolve part of the cerium; through an impurity precipitation process, common non-rare earth impurities such as aluminum, iron, uranium, thorium, and fluorine in the rare earth liquid are precipitated into impurities in a reaction system with a relatively low pH value; through an impurity adsorption process, when the pH value reaches the impurity precipitation end point, the cerium-based material forms an adsorption material with a large specific surface area, which effectively adsorbs the impurity precipitate in the liquid phase; through a solid-liquid separation process, the rare earth liquid and the solid that has adsorbed the impurities are separated into solid and liquid by a simple method such as suction filtration or filter press, to obtain the low-impurity rare earth liquid. The method provided in this embodiment prepares a low-impurity rare earth liquid, which is beneficial to the subsequent rare earth extraction and separation process, increases the organic phase extraction and separation capacity, and effectively reduces the extraction and separation cost; and the prepared low-impurity rare earth liquid has lower uranium and thorium contents, reducing the radioactivity of the product.
[0057] The specific implementation modes of the present invention are further described below through examples.
[0058] Example 1: When the rare earth feed liquid containing impurities is a rare earth chloride feed liquid obtained by dissolving the yttrium-rich rare earth ore from the southern mine with hydrochloric acid, the following method steps are used to prepare a low-impurity rare earth feed liquid:
[0059] (1) Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction;
[0060] (2) Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction;
[0061] (3) Adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurities;
[0062] (4) Solid-liquid separation: The low-impurity rare earth liquid is obtained by performing solid-liquid separation on the rare earth liquid and the solid that has adsorbed impurities.
[0063] The rare earth solution containing impurities is a rare earth chloride solution obtained by dissolving yttrium-rich rare earth ore from a southern mine in hydrochloric acid, with a concentration of 1.55 mol / L and a pH value of <1.
[0064] The cerium-based material is composed of cerium dioxide and cerium dioxide-non-cerium rare earth composite material, with cerium dioxide accounting for 20%. The reducing agent is composed of citric acid and thiourea, and the molar ratio of the cerium-based material to the reducing agent is 10:1. The temperature of the redox reaction is 25°C and the reaction time is 24h.
[0065] In step (2), the precipitation reaction temperature is 25° C., the precipitation reaction time is 12 h, and the pH value of the reaction system is controlled between 1 and 3.5.
[0066] In step (3), the endpoint pH value of the precipitation reaction is 3.5, the reaction temperature for maintaining the endpoint pH value of the precipitation reaction and continuing the reaction is 25° C., and the reaction time is 12 h.
[0067] By performing solid-liquid separation by suction filtration, a low-impurity rare earth feed liquid with a low impurity content as shown in Table 1 can be prepared.
[0068] Table 1 Rare earth and impurity concentrations in initial and prepared rare earth solutions
[0069]
[0070] Example 2 When the rare earth feed liquid containing impurities is a nitrate rare earth feed liquid obtained by dissolving yttrium rare earth ore in a southern mine with nitric acid, the following method steps are used to prepare a low-impurity rare earth feed liquid
[0071] (1) Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction;
[0072] (2) Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction;
[0073] (3) Adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurities;
[0074] (4) Solid-liquid separation: The low-impurity rare earth liquid is obtained by performing solid-liquid separation on the rare earth liquid and the solid that has adsorbed impurities.
[0075] The rare earth solution containing impurities is a nitrate rare earth solution obtained by dissolving yttrium rare earth ore in a southern mine with nitric acid, with a concentration of 1.36 mol / L and a pH value of <2.
[0076] The cerium-based material is composed of cerium hydroxide and cerium dioxide-enriched slag, and the cerium hydroxide and cerium dioxide account for 50% in total. The reducing agent is composed of urea and hydroxylamine hydrochloride, and the molar ratio of the cerium-based material to the reducing agent is 10:3. The temperature of the redox reaction is 55° C. and the reaction time is 15 hours.
[0077] In step (2), the precipitation reaction temperature is 55° C., the precipitation reaction time is 5 h, and the pH value of the reaction system is controlled between 1 and 3.8.
[0078] In step (3), the endpoint pH value of the precipitation reaction is 3.8, the reaction temperature for maintaining the endpoint pH value of the precipitation reaction and continuing the reaction is 55° C., and the reaction time is 5 hours.
[0079] By performing solid-liquid separation by natural filtration, a low-impurity rare earth feed liquid with a low impurity content as shown in Table 2 can be prepared.
[0080] Table 2 Rare earth and impurity concentrations in initial and prepared rare earth solutions
[0081]
[0082] Example 3 When the rare earth feed liquid containing impurities is a chloride rare earth feed liquid obtained by dissolving a light rare earth ore with hydrochloric acid, the following method steps are used to prepare a low-impurity rare earth feed liquid
[0083] (1) Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction;
[0084] (2) Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction;
[0085] (3) Adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurities;
[0086] (4) Solid-liquid separation: The low-impurity rare earth liquid is obtained by performing solid-liquid separation on the rare earth liquid and the solid that has adsorbed impurities.
[0087] The rare earth solution containing impurities is a rare earth chloride solution obtained by dissolving a light rare earth ore in hydrochloric acid, with a concentration of 1.77 mol / L and a pH value of <1.
[0088] The cerium-based material is composed of slag enriched with cerium hydroxide, with cerium hydroxide accounting for 40%. The reducing agent is composed of hydrogen peroxide, with a molar ratio of the cerium-based material to the reducing agent of 10:5. The temperature of the redox reaction is 85° C., and the reaction time is 4 hours.
[0089] In step (2), the precipitation reaction temperature is 85° C., the precipitation reaction time is 2 h, and the pH value of the reaction system is controlled between 1 and 4.0.
[0090] In step (3), the endpoint pH value of the precipitation reaction is 4.0, the reaction temperature for maintaining the endpoint pH value of the precipitation reaction and continuing the reaction is 85° C., and the reaction time is 2 h.
[0091] By performing solid-liquid separation by filter pressing, a low-impurity rare earth feed liquid with a low impurity content as shown in Table 3 can be prepared.
[0092] Table 3 Rare earth and impurity concentrations in initial and prepared rare earth solutions
[0093]
[0094] It can be clearly seen from the results in Tables 1-3 that the low-impurity rare earth solution obtained by the method provided by the embodiment of the present invention has an impurity level at least one order of magnitude lower than that of the rare earth solution obtained by the current acid dissolution process. Therefore, the low-impurity rare earth solution does not need to be treated separately for impurities.
[0095] The method described in the present invention is not limited to the specific embodiments described. The above embodiments are only examples of the present invention. The present invention can also be implemented in other specific ways or other specific forms without departing from the gist or essential features of the present invention. Therefore, the described embodiments should be regarded as illustrative rather than restrictive in any respect. The scope of the present invention should be described by the attached claims, and any changes equivalent to the intent and scope of the claims should also be included in the scope of the present invention.
Claims
1. A method for preparing a low-impurity rare earth liquid using a cerium-based material, characterized in that: The method comprises the following steps: S1. Redox: adding cerium-based materials and reducing agents to the rare earth liquid containing impurities to carry out redox reaction; S2. Precipitating impurities: adjusting the pH value of the reaction system to precipitate impurities through precipitation reaction; S3, adsorption of impurities: maintaining the pH value at the end point of the precipitation reaction and continuing the reaction to complete the adsorption of impurity precipitation; S4, solid-liquid separation: The low-impurity rare earth feed liquid is obtained by performing solid-liquid separation on the rare earth feed liquid and the solid that has adsorbed impurities.
2. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: The rare earth liquid containing impurities is a hydrochloric acid and / or nitric acid rare earth solution, and the impurities in the rare earth liquid containing impurities include one or more of aluminum, iron, fluorine, uranium, and thorium.
3. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: The concentration of rare earth elements in the rare earth solution containing impurities is 0.1-2.5 mol / L; the pH value of the rare earth solution containing impurities is less than 5.
5.
4. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: The cerium-based material is selected from one or more of cerium dioxide, cerium hydroxide, cerium dioxide-non-cerium rare earth composite material, cerium hydroxide-non-cerium rare earth composite material, cerium dioxide-non-rare earth metal composite material, cerium hydroxide-non-rare earth metal composite material, slag containing cerium dioxide, and slag containing cerium hydroxide.
5. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: The reducing agent includes one or more of citric acid, thiourea, urea, hydroxylamine hydrochloride, hydrogen peroxide, iron powder, and glucose.
6. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: The molar ratio of the cerium-based material to the reducing agent is 10:1 to 1:
10.
7. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: In step S1, the temperature of the redox reaction is 10-100°C, and the reaction time is 0.5-100h.
8. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: In step S2, the pH value of the reaction system is regulated by adding a pH regulating agent; The pH value regulating reagent includes one or more of sodium hydroxide, ammonia water, ammonium bicarbonate, sodium bicarbonate, ammonium carbonate, sodium carbonate, rare earth hydroxide, composite rare earth hydroxide, and rare earth oxide.
9. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 1, characterized in that: In step S2, the pH value of the reaction system is controlled between 1 and 5; The temperature of the precipitation reaction is 10-100° C., and the precipitation reaction time is 0.5-100 h.
10. A method for preparing a low-impurity rare earth liquid using a cerium-based material according to any one of claims 1 to 9, characterized in that: In step S3, the precipitation reaction end point pH value is 2.5-5.
11. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 10, characterized in that: In step S3, the reaction temperature for continuing the reaction while maintaining the pH value at the end point of the precipitation reaction is 10 to 100° C., and the reaction time is 0.5 to 24 h.
12. The method for preparing a low-impurity rare earth liquid using a cerium-based material according to claim 10, characterized in that: In step S4, the solid-liquid separation method includes natural filtration, suction filtration or pressure filtration.
Citation Information
Patent Citations
Method for performing water treatment by using tetravalent cerium
CN101948195A
Method for recovering rare earth from ionic type rare earth crude ore
CN102190325A
Nano adsorbent for removing arsenic, stibium and fluorin in wastewater as well as preparation method and regeneration method of nano adsorbent
CN103341353A
Method for removing cerium and non-rare earth impurities from rare earth feed liquid
CN111996396A
Recovery of tantalum and / or niobium from metalfluoride containing materials and ore residues with use of sulfuric acid roasting
EP0834584A1