Metal part pretreatment method

The composite film is formed through silane, zirconium and silicon zirconium pretreatment liquid, which solves the problems of environmental pollution and insufficient corrosion resistance of the traditional pretreatment process, and achieves high corrosion resistance of metal parts and improved coating adhesion. Silicon zirconium The treatment effect is the most significant.

CN118745570APending Publication Date: 2024-10-08CHENGDU DEWEI PETROLEUM TECH SERVICE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410758790.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional metal pretreatment processes such as phosphating and chromate passivation cause environmental pollution and are difficult to effectively improve the corrosion resistance of metal parts. Research and develop efficient, energy-saving, and environmentally friendly pretreatment technologies to replace traditional methods.

Method used

Silane, zirconium and silicon-zirconium pretreatment liquids are used to form a composite film. Through pre-degreasing, rust removal, water washing, film formation and drying steps, the corrosion resistance and coating adhesion of metal parts are significantly improved.

Benefits of technology

The corrosion resistance and coating adhesion of metal parts are significantly improved. The composite film itself has excellent corrosion resistance and provides effective anti-corrosion protection. The silicon zirconization treatment has the most significant effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745570A_ABST
    Figure CN118745570A_ABST
Patent Text Reader

Abstract

The invention provides a metal part pretreatment method. The metal part pretreatment method comprises the steps that S1, pretreatment liquid, degreasing liquid and rust removal liquid are prepared; the pretreatment liquid is one of silane pretreatment liquid, zirconium pretreatment liquid and silicon-zirconium pretreatment liquid; s2, performing pre-degreasing and degreasing by using degreasing fluid; s3, the degreased metal part is washed with water; s4, rust removal is conducted through rust removal liquid; s5, the derusted metal part is sequentially subjected to water washing and pure water washing; s6, the pretreatment liquid is used for preparing a pretreatment film on the surface of the metal part; and S7, the metal part is dried. According to the invention, the corrosion resistance of the metal substrate and the adhesive force of the coating are obviously improved, and the composite film has excellent corrosion resistance, so that effective anti-corrosion protection is provided for metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal anticorrosion, and in particular to a metal part pretreatment method. Background Art

[0002] The corrosion of metal materials has caused great damage to the national economy and has also seriously affected production safety and environmental protection. Metal pretreatment plus organic coating is one of the most effective measures for metal corrosion prevention, but the traditional pretreatment process uses phosphating and chromate passivation, which causes serious environmental pollution and is now restricted. It is urgent to research and develop efficient, energy-saving and environmentally friendly pretreatment technology to replace phosphating. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a metal part pretreatment method, which can improve the corrosion resistance of the metal part, and is specifically achieved through the following technical solutions:

[0004] The present invention provides a metal part pretreatment method, comprising the following steps:

[0005] S1, solution preparation; the solution includes a pretreatment liquid, a degreasing liquid and a rust removal liquid; the pretreatment liquid is one of a silane pretreatment liquid, a zirconization pretreatment liquid and a silicon zirconium pretreatment liquid;

[0006] S2, using the degreasing liquid to perform pre-degreasing and degreasing on the metal parts in sequence;

[0007] S3, washing the degreased metal parts with water;

[0008] S4, using the rust removal liquid to remove rust from metal parts;

[0009] S5, washing the rust-removed metal parts with water and pure water in sequence;

[0010] S6, using the pretreatment liquid to prepare a pretreatment film on the surface of the metal part;

[0011] S7. Drying the metal parts.

[0012] Optionally or preferably, the silane pretreatment liquid is configured by the following steps: dissolving 3-5wt% of a silane coupling agent in a 4-6wt% ethanol solution, adding pure water while stirring, continuing stirring for more than 60 minutes, then adding 1-2wt% of a silicone resin, 0.1-1wt% of triethanolamine and 0.1-0.2wt% of a film-forming aid in sequence, and finally adding pure water and stirring evenly to obtain a silane pretreatment liquid.

[0013] Optionally or preferably, the zirconization pretreatment liquid is prepared by the following steps: dissolving 3-5wt% of fluorozirconic acid in pure water, dissolving 1-3wt% of sodium citrate, 0.3-0.8wt% of sodium tetraborate, 5-12wt% of magnesium nitrate, 3-5wt% of aluminum sulfate and 0.1-0.3wt% of film-forming promoter in sequence under stirring, adding pure water, adjusting the pH value to 4.0-4.5 with 1mol / L sodium hydroxide, and stirring evenly to obtain the zirconization pretreatment liquid.

[0014] Optionally or preferably, the silicon zirconium pretreatment liquid is configured by the following steps: dissolving 2-5wt% of a silane coupling agent in an ethanol solution, adding pure water under stirring, then adding 0.8-2wt% of a silicone resin, 0.1-1wt% of triethanolamine and 0.1-0.2wt% of a film-forming aid A, and stirring evenly to obtain a solution A; dissolving 1.5-4.5wt% of fluorozirconic acid in pure water, adding 1-2wt% of sodium citrate, 0.1-1wt% of sodium tetraborate, 3-8wt% of magnesium nitrate, 1-5wt% of aluminum sulfate and 0.1-0.3wt% of a film-forming promoter B in sequence under stirring, and stirring evenly to obtain a solution B; while stirring, slowly adding the B solution to the A solution, adding pure water, stirring for more than 60 minutes, and adjusting the pH value to 4.0-4.5 with 1mol / L of sodium hydroxide, and stirring evenly to obtain a silicon zirconium pretreatment liquid.

[0015] Optionally or preferably, the degreasing liquid is prepared by the following steps: 1-3wt% sodium carbonate, 1-2wt% sodium tripolyphosphate, 0.1-0.3wt% OP-10 emulsifier and 1-3wt% triacetate ammonium oleate soap are dissolved in pure water in sequence, and the degreasing liquid is obtained after stirring evenly.

[0016] Optionally or preferably, the rust removing liquid is prepared by the following steps: slowly adding 2-5wt% sulfuric acid into pure water, then adding 0.5-2wt% thiourea, and stirring evenly to obtain the rust removing liquid.

[0017] Optionally or preferably, steps S2-S6 are all performed at room temperature; the drying temperature in step S7 is 80°C

[0018] Optionally or preferably, the pre-degreasing and degreasing in step S2 take no less than 10 minutes; the film forming time in step S6 is no less than 5 minutes; and the drying time in step S7 is no less than 20 minutes.

[0019] Based on the above technical solution, the following technical effects can be produced:

[0020] The present invention provides a metal part pretreatment method, which significantly improves the corrosion resistance and coating adhesion of the metal substrate by forming a composite film on the surface of the metal substrate, and the composite film itself has excellent corrosion resistance, thereby providing effective anti-corrosion protection for the metal. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0022] Figure 1 The metal appearance morphology before and after the neutral salt spray test;

[0023] Figure 2 It is the potentiodynamic polarization curve diagram in the electrochemical test experiment;

[0024] Figure 3 This is the AC impedance spectrum in the electrochemical test experiment;

[0025] Figure 4 Equivalent circuit diagram used for AC impedance spectrum fitting in electrochemical test experiments;

[0026] Figure 5 This is a microscopic morphology of the metal surface. DETAILED DESCRIPTION

[0027] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the following embodiments, a 50 mm × 50 mm × 2 mm Q235 cold-rolled steel test piece is used as the test metal part.

[0030] Embodiment 1:

[0031] A metal part pretreatment method provided in this embodiment includes the following steps:

[0032] S1. Solution configuration:

[0033] A. Prepare degreasing liquid;

[0034] Specifically, 2g of sodium carbonate, 1.5g of sodium tripolyphosphate, 0.2g of OP-10 emulsifier, and 2g of triacetamide oleic acid soap were dissolved in 60g of pure water in sequence, and pure water was added to 100g, and stirred evenly for later use;

[0035] B. Prepare rust removal liquid;

[0036] Specifically, under stirring, slowly add 2 ml of sulfuric acid to 60 g of pure water, then add 1 g of thiourea, add pure water to 100 g, stir evenly and set aside;

[0037] C. preparing a silane pretreatment liquid as a film-forming pretreatment liquid;

[0038] Specifically, 3.5 g of silane coupling agent was dissolved in 5 g of ethanol solution, 50 g of pure water was added under stirring, and stirring was continued for more than 60 minutes. Then 1.5 g of silicone resin, 0.5 g of triethanolamine, and 0.1 g of film-forming aid A were added in sequence, and finally pure water was added to 100 g, and stirred evenly. The silane pretreatment liquid was prepared according to the ratio of silane liquid: pure water = 1:49; wherein the silane coupling agent was KH550 silane coupling agent of Yunsheng Chemical Co., Ltd.; and the silicone resin was SH-95 silicone resin of Hubei Xinsihai Chemical Co., Ltd.

[0039] S2. The metal parts for the test are polished with 400#, 600#, 800# and 1000# sandpapers in sequence, and the above-mentioned degreasing liquid is used to pre-degrease and degrease the metal parts in sequence for 10 minutes.

[0040] S3, washing the degreased metal parts with water;

[0041] S4, using the above rust removal liquid to remove rust from metal parts;

[0042] S5, washing the rust-removed metal parts with water and pure water in sequence;

[0043] S6, using a silane pretreatment liquid to silanize the surface of the metal part for 5 minutes to form a silanization pretreatment film;

[0044] S7. Place the metal parts in an oven at 80°C and dry for 20 minutes.

[0045] Embodiment 2:

[0046] The metal part pretreatment method provided in this embodiment has the following differences compared with the embodiment 1:

[0047] This embodiment configures the zirconization pretreatment liquid as the film-forming pretreatment liquid;

[0048] Specifically, 3.6 g of fluorozirconic acid was dissolved in 60 g of pure water, and 2 g of sodium citrate, 0.5 g of sodium tetraborate, 8 g of magnesium nitrate, 4 g of aluminum sulfate, and 0.2 g of film-forming promoter B were dissolved in sequence under stirring, and pure water was added to 100 g, and stirred evenly, and the mixture was prepared according to the ratio of zirconization liquid: pure water = 1:49, and the pH value was adjusted to 4.0-4.5 with 1 mol / L of sodium hydroxide to serve as a zirconization pretreatment liquid; wherein, the fluorozirconic acid was analytically pure fluorozirconic acid produced by Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0049] In this embodiment, a zirconization pretreatment liquid is used to zirconize the surface of the metal part for 5 minutes to form a zirconization pretreatment film.

[0050] In this embodiment, after the metal part is zirconized, it is washed with water, washed with pure water, and then dried.

[0051] Embodiment 3:

[0052] The metal part pretreatment method provided in this embodiment has the following differences compared with the embodiment 1:

[0053] This embodiment configures a silicon-zirconium pretreatment liquid as a film-forming pretreatment liquid;

[0054] Specifically, 3 grams of silane coupling agent is dissolved in 5 grams of ethanol solution, 30 grams of pure water is added under stirring, 1.2 grams of silicone resin, 0.5 grams of triethanolamine, and film-forming aid A are added, and the mixture is stirred evenly to obtain solution A; 3.1 grams of fluorozirconic acid is dissolved in 40 grams of pure water, 1.6 grams of sodium citrate, 0.5 grams of sodium tetraborate, 6 grams of magnesium nitrate, 2.5 grams of aluminum sulfate, and 0.2 grams of film-forming promoter B are added in sequence under stirring, and the mixture is stirred evenly to obtain solution B; under stirring, solution B is slowly added to solution A, pure water is added to 100 grams, and the mixture is stirred for more than 60 minutes, and the mixture is prepared according to the ratio of silicon zirconium liquid to pure water = 1:49, and the pH value is adjusted to 4.0-4.5 with 1 mol / L of sodium hydroxide to serve as a silicon zirconium pretreatment solution.

[0055] In this embodiment, a silicon zirconium pretreatment liquid is used to siliconize the surface of the metal part for 5 minutes to form a silicon zirconium pretreatment film.

[0056] In this embodiment, after the metal parts are siliconized, they are washed with water, washed with pure water, and then dried.

[0057] In order to illustrate the effect of the preprocessing method proposed in the present invention, a number of performance tests are performed on the above embodiments, and some experimental results are listed as follows:

[0058] 1. Neutral salt spray test:

[0059] Neutral salt spray test is one of the most effective methods to evaluate the corrosion resistance of materials, with the advantages of being intuitive, accurate and efficient. This experiment is carried out in accordance with GB / T 1771-2007 "Determination of neutral salt spray resistance of paints and varnishes". The corrosion solution is 5% NaCl solution, and the temperature in the test chamber is 35℃±2.

[0060] like Figure 1 As shown, it is a comparison diagram before and after the salt spray test of the same test metal parts after different pretreatment methods; in the figure, the upper row is the surface morphology of the sample before the experiment, from left to right they belong to the unpretreated sample, Example 1, Example 2 and Example 3 respectively; the lower row is the surface morphology of the sample after 2 hours of neutral salt spray test, from left to right they belong to the unpretreated sample, Example 1, Example 2 and Example 3 respectively.

[0061] like Figure 1 As shown in the upper middle row, the surface morphology of the sample after silanization has no obvious change, and the surface of the sample after zirconization or silicon zirconization presents a uniform light blue color; Figure 1 As shown in the lower middle row, the surface of the sample that has not been pretreated is severely corroded, and almost the entire surface is corroded; the corrosion level of the sample that has been silanized is reduced by about 30%, and the corrosion level of the sample that has been zirconized is reduced by about 40%. The sample that has been treated with silicon zirconization has red rust only on the edges and a few areas, the corrosion area does not exceed 10%, and there is basically no pitting.

[0062] The results of the neutral salt spray test show that the pretreatment method proposed in the present invention improves the corrosion protection effect of metal parts, and the corrosion resistance of the surface of the silicon zirconization treated sample (Example 3) is the best.

[0063] 2. Electrochemical experiment:

[0064] In this experiment, a VersaSTAT 3 electrochemical workstation was used to perform polarization curve and AC impedance tests. The test used a three-electrode system, with the metal sample as the working electrode, the platinum electrode as the counter electrode, and the saturated calomel electrode as the reference electrode. The test was carried out in an electrolytic cell with a length, width, and height of 10 cm respectively. There was a circular hole with an area of ​​1 cm on one side of the electrolytic cell, and the sample was in contact with the solution through the circular hole. The test solution was a 3% NaCl solution, the temperature was 25°C, the potential scanning amplitude of the polarization curve was E±0.3V (E is the self-corrosion potential), the scanning speed was 1mV / s, and the AC impedance test frequency range was 10 5 -10 -2 Hz, and the AC excitation signal amplitude is 10mV.

[0065] Figure 2 The potentiodynamic polarization curves of the same test metal parts after different pretreatment methods are shown in Figure 2. Figure 2As shown, the polarization curves after silanization, zirconization and silicon zirconization treatments obviously move in the positive direction. From thermodynamics, we know that the more positive the potential, the smaller the corrosion tendency of the material, indicating that the above three embodiments all reduce the tendency of metal to electrochemical corrosion. Moreover, among them, silicon zirconization moves the most in the positive direction, indicating that the tendency of electrochemical corrosion after silicon zirconization treatment is the smallest.

[0066] As shown in Table 1, the electrochemical polarization curve corrosion parameters obtained by the Tafel curve extrapolation method are:

[0067] Table 1

[0068] Sample Ecorr(mV) <![CDATA[Icorr(A·cm -2 )]]> βa(mv / dec) βc(mv / dec) blank -0.7283 <![CDATA[3.495×10 -9 ]]> 65.1 188.1 Silanization -0.6103 <![CDATA[9.364×10 -8 ]]> 78.2 178.2 Zirconation -0.6343 <![CDATA[8.297×10 -8 ]]> 80.3 192.2 Silicon zirconium -0.5699 <![CDATA[9.295×10 -7 ]]> 82.5 189.9

[0069] Among them, the corrosion current density reflects the corrosion rate of the material. It can be seen from Table 1 that the corrosion rates of the samples treated by this method are all reduced, indicating that this method effectively reduces the corrosion rate of the material and inhibits the occurrence of surface corrosion of the metal material. Among them, the corrosion rate of silicon zirconium (Example 3) is reduced the most, and the corrosion current density is only 1 / 38 of that of the untreated sample, which shows that the protection performance of the silicon zirconium film is the best.

[0070] Figure 3 is the AC impedance spectrum of the sample in 3% NaCl solution, such as Figure 3 As shown in the figure, the impedance spectra of the blank sample without pretreatment and the sample treated by this method both show a "suppressed" semicircular impedance arc. The impedance arc represents the relaxation process of the metal interface charge transfer resistance and the double layer resistance and capacitance, and its radius reflects the size of the corrosion resistance. Figure 3 It can be seen that the capacitive reactance arcs of the blank sample, silanized sample, zirconized sample and siliconized zirconized sample increase in turn, indicating that their corrosion resistance increases in turn.

[0071] Figure 4 This is the equivalent circuit diagram used for the impedance spectrum fitting mentioned above. The electrochemical data after fitting are shown in Table 2:

[0072] Table 2

[0073] Sample <![CDATA[Rs(Ωcm 2 )]]> <![CDATA[Rct(Ωcm 2 )]]> <![CDATA[Cdl(μFcm -2 )]]> n blank 34 805 89 0.66 Silanization 29 2253 45 0.60 Zirconation 34 2453 81 0.98 Silicon zirconium 29 5152 68 0.90

[0074] Among them, Rs in the table is the solution resistance, which is the resistance of the solution between the Luggin capillary of the reference electrode and the sample electrode; Rct is the charge transfer resistance, which characterizes the resistance of the electrochemical corrosion reaction of the sample.

[0075] As shown in Table 2, the surface corrosion resistance of the sample after silane and zirconization is about 3 times that of the untreated sample, while the surface corrosion resistance after silicon zirconium treatment is 6.4 times the original. Therefore, silane and zirconization both improve the corrosion resistance of the metal surface to a certain extent, while silicon zirconium treatment greatly improves the corrosion resistance of the material surface; Cdl in the phase angle element CPE is the double layer capacitance. Table 2 shows that the double layer capacitance on the surface of the silane film and silicon zirconium film is relatively small. This is because the silane molecules with larger volume and smaller dielectric constant replace the water molecules adsorbed on the surface of the substrate, resulting in a decrease in the double layer capacitance of the sample surface; n in CPE represents the roughness of the substrate surface. After zirconization and silicon zirconization, the n value of the metal surface is significantly increased, indicating that the material has improved the surface roughness after zirconization or silicon zirconization.

[0076] 3. Coating adhesion test:

[0077] Improving coating adhesion is one of the main purposes of metal pretreatment process.

[0078] This experiment uses the Accutester pull-off tester ACT-20 and is tested in accordance with the GB / T5210-2006 "Pull-off adhesion test for paints and varnishes". The sample is sprayed with a 60μm thick epoxy primer, dried at 80℃ for 20 minutes, and then cured at room temperature for 24 hours.

[0079] As shown in Table 3, the adhesion test results of this experiment are:

[0080] Table 3

[0081] Sample Adhesion / MPa blank 4.12 Silanization 11.32 Zirconation 10.56 Silicon zirconium 11.76

[0082] As shown in Table 3, the adhesion of the coating treated by this method is significantly improved. Generally speaking, a coating adhesion of 5MPa can meet general coating requirements. The adhesion of the coating treated by the present invention is greater than 10MPa, which fully meets the coating adhesion requirements.

[0083] 4. Microscopic morphology analysis experiment:

[0084] In this experiment, a SU3500 (Hitachi) scanning electron microscope was used to observe the samples. Figure 5 The following are the surface micrographs of the untreated and pretreated samples.

[0085] Figure 5 (a) is the microscopic morphology of the blank sample without pretreatment. It can be seen that its surface is uneven, with obvious grinding marks and a lot of debris. These debris not only affect the adhesion of the subsequent coating, but also reduce the corrosion resistance of the substrate.

[0086] Figure 5(b) is a microscopic morphology image of the sample (Example 1) after silanization treatment, and it can be seen that the surface is obviously flat and there is basically no debris.

[0087] Figure 5 (c) is a microscopic morphology of the sample (Example 2) after zirconization treatment. It can be seen that the surface is relatively flat and cracked. This is because Zr(OH)2 is formed during the electrochemical corrosion of the zirconium salt with the substrate, and Zr(OH)2 is dried and dehydrated. Although the cracked surface of the zirconized film can increase the specific surface area and improve the adhesion of the coating, the high porosity reduces the corrosion resistance of the film itself to a certain extent. This is the reason why the zirconized film is severely pitted in the salt spray test.

[0088] Figure 5 (d) is a microscopic morphology of the sample (Example 3) treated with silicon zirconization. It can be seen that the silicon zirconization film is flat, dense, without debris and cracks. The Si-OH groups formed by the hydrolysis of silane are adsorbed on the surface of the substrate to form Si-O-Fe bonds, and the excess Si-OH groups form a Si-O-Si three-dimensional network structure on the surface of the substrate. At the same time, Zr(OH)2 formed by zirconium salt is mixed with a large amount of Si-O-Si three-dimensional network structure during the precipitation process. The filling and interconnection of the Si-O-Si three-dimensional network structure reduces the porosity of the silicon zirconization film, increases the thickness of the composite film, and improves the corrosion resistance of the composite film.

[0089] In summary, the present invention has the following advantages:

[0090] 1. Silanization, zirconization and silicon zirconization pretreatment processes can effectively improve the corrosion resistance of the bare film, and silicon zirconization pretreatment has the best effect;

[0091] 2. The adhesion of the coating after pretreatment is greater than 10MPa, which fully meets the general coating adhesion requirements;

[0092] 3. The surface of the sample after pretreatment is smoother, which improves the corrosion resistance of the composite film itself.

[0093] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A metal part pretreatment method, characterized in that: The following steps are involved: S1, solution preparation; the solution includes a pretreatment liquid, a degreasing liquid and a rust removal liquid; the pretreatment liquid is one of a silane pretreatment liquid, a zirconization pretreatment liquid and a silicon zirconium pretreatment liquid; S2, using the degreasing liquid to perform pre-degreasing and degreasing on the metal parts in sequence; S3, washing the degreased metal parts with water; S4, using the rust removal liquid to remove rust from metal parts; S5, washing the rust-removed metal parts with water and pure water in sequence; S6, using the pretreatment liquid to prepare a pretreatment film on the surface of the metal part; S7. Drying the metal parts.

2. A metal part pretreatment method according to claim 1, characterized in that: The silane pretreatment liquid is prepared by the following steps: dissolving 3-5wt% of a silane coupling agent in a 4-6wt% ethanol solution, adding pure water under stirring, continuing to stir for more than 60 minutes, then sequentially adding 1-2wt% of an organic silicone resin, 0.1-1wt% of triethanolamine and 0.1-0.2wt% of a film-forming aid, and finally adding pure water and stirring evenly to obtain the silane pretreatment liquid.

3. A metal part pretreatment method according to claim 1, characterized in that: The zirconization pretreatment liquid is prepared by the following steps: dissolving 3-5wt% of fluorozirconic acid in pure water, dissolving 1-3wt% of sodium citrate, 0.3-0.8wt% of sodium tetraborate, 5-12wt% of magnesium nitrate, 3-5wt% of aluminum sulfate and 0.1-0.3wt% of film-forming accelerator in sequence under stirring, adding pure water, adjusting the pH value to 4.0-4.5 with 1mol / L of sodium hydroxide, and stirring evenly to obtain the zirconization pretreatment liquid.

4. A metal part pretreatment method according to claim 1, characterized in that: The silicon zirconium pretreatment liquid is prepared by the following steps: dissolving 2-5wt% of a silane coupling agent in an ethanol solution, adding pure water under stirring, then adding 0.8-2wt% of an organic silicone resin, 0.1-1wt% of triethanolamine and 0.1-0.2wt% of a film-forming aid A, and stirring evenly to obtain a solution A; dissolving 1.5-4.5wt% of fluorozirconic acid in pure water, adding 1-2wt% of sodium citrate, 0.1-1wt% of sodium tetraborate, 3-8wt% of magnesium nitrate, 1-5wt% of aluminum sulfate and 0.1-0.3wt% of a film-forming accelerator B in sequence under stirring, and stirring evenly to obtain a solution B; and slowly adding the B solution to the A solution under stirring, adding pure water, stirring for more than 60 minutes, adjusting the pH value to 4.0-4.5 with 1mol / L of sodium hydroxide, and stirring evenly to obtain a silicon zirconium pretreatment liquid.

5. A metal part pretreatment method according to claim 1, characterized in that: The degreasing liquid is prepared by the following steps: 1-3wt% sodium carbonate, 1-2wt% sodium tripolyphosphate, 0.1-0.3wt% OP-10 emulsifier and 1-3wt% triacetamide oleic acid soap are sequentially dissolved in pure water, and the degreasing liquid is obtained after being stirred evenly.

6. A metal part pretreatment method according to claim 1, characterized in that: The rust removing liquid is prepared by the following steps: slowly adding 2-5wt% sulfuric acid into pure water, then adding 0.5-2wt% thiourea, and stirring evenly to obtain the rust removing liquid.

7. A metal part pretreatment method according to claim 1, characterized in that: The steps S2-S6 are all performed at room temperature; the drying temperature in the step S7 is 80°C.

8. A metal part pretreatment method according to claim 7, characterized in that: The pre-degreasing and degreasing in step S2 take no less than 10 minutes; the film forming time in step S6 is no less than 5 minutes; and the drying time in step S7 is no less than 20 minutes.

Citation Information

Patent Citations

  • Silane finishing agent at surface of galvanized steel sheet and preparation method thereof

    CN103088328A

  • Coating pretreatment technology with acid pickling process

    CN106086907A

  • Metal surface multifunctional environment-friendly type nanometer ceramization liquid and preparing method and using method thereof

    CN109321908A