Method for rapidly preparing lyocell cross-linked short fibers

By rotating, stirring, and heating the fiber and the cross-linking agent solution in the reaction vessel, the preparation process of lyocell cross-linked short fibers is simplified, the problems of high equipment investment and high energy consumption in the existing technology are solved, and low energy consumption is achieved , efficient cross-linking effect and good anti-fibrillation performance.

CN118745662APending Publication Date: 2024-10-08YIBIN SILIYA TECHNOLOGY INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410917477.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When preparing lyocell cross-linked short fibers with the existing technology, equipment investment and energy consumption are high, and the process steps are numerous, which leads to an increase in production costs, and the fibers are prone to fibrillation, which affects downstream applications.

Method used

After cutting the fiber filaments into short fibers, the cross-linking agent solution is rotated, stirred and heated in a reaction vessel to carry out the cross-linking reaction, which simplifies the process, reduces equipment investment and energy consumption, and improves the utilization rate of the cross-linking agent.

Benefits of technology

This method achieves rapid and low-energy preparation of lyocell cross-linked short fibers with good anti-fibrillation properties, simplifies the process steps, reduces equipment costs and energy consumption, and improves the utilization rate of the cross-linking agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745662A_ABST
    Figure CN118745662A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fiber preparation, and particularly provides a method for rapidly preparing lyocell cross-linked short fibers, which comprises the following steps: S1, cutting fiber filaments into short fibers; s2, preparing a cross-linking agent solution; s3, simultaneously putting the short fibers and the cross-linking agent solution into a reaction container, rotating, stirring and heating, and carrying out cross-linking reaction; s4, after the cross-linking reaction is finished, washing with water to obtain lyocell cross-linked short fibers with fibrillation resistance; according to the invention, the short fibers and the cross-linking agent solution are put into the reaction container together for cross-linking reaction, the reaction container continuously rotates, stirs and heats during the cross-linking reaction, and multiple padding in the cross-linking process in the prior art is not needed, and meanwhile, the cross-linking agent always reacts with the fibers before being discharged; the utilization rate of the cross-linking agent is fully improved; and moreover, the used equipment and preparation steps are optimized and reduced, the equipment cost and the equipment energy consumption are effectively reduced, and the Lyocell short fibers with good fibrillation resistance can be efficiently and quickly prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber preparation, and specifically provides a method for quickly preparing lyocell cross-linked staple fibers. Background Art

[0002] Lyocell fiber is a highly crystalline, highly oriented, low energy consumption, pollution-free, and naturally degradable cellulose fiber with superior performance and wide applications. However, due to the weak lateral bonding force between the microfibers of Lyocell fiber, it is very easy to fibrillate when wet. Severe fibrillation will lead to difficulties in downstream spinning and non-woven fabric production, and downstream applications will be limited.

[0003] In order to overcome the problem of fibrillation of lyocell fibers, it is necessary to perform a cross-linking post-treatment on the fibers to enhance their anti-fibrillation properties. Therefore, the preparation of lyocell cross-linked fibers requires adding a cross-linking process to the conventional production process. At present, the preparation of lyocell cross-linked staple fibers usually involves immersing the washed fiber filament bundles in a cross-linking agent solution or spraying the cross-linking agent solution on the fiber filament bundles, and then entering a high-temperature device for cross-linking reaction. The filament bundles after the cross-linking reaction are washed, oiled, and dried, and then cut into staple fibers to obtain cross-linked staple fibers.

[0004] For example, in the prior art:

[0005] (1) Chinese patent CN113265788A discloses a method and device for preparing Lyocell cross-linked fibers. In this patent, a cross-linking liquid formed by mixing a cross-linking agent solution and a catalyst solution is sprayed on a fiber ribbon, and the fiber ribbon is subjected to high-temperature curing treatment after extrusion to obtain Lyocell cross-linked fibers. This patent has many cross-linking steps, requires a large amount of equipment investment, and has a high temperature curing reaction temperature and high energy consumption, which will significantly increase production costs;

[0006] (2) Chinese patent CN113293549A discloses a two-stage method and apparatus for preparing crosslinked fibers. The patent treats fiber ribbons with a crosslinking agent solution and a catalyst solution respectively, and then solidifies them to obtain crosslinked fibers. Although the hydrolysis and self-polymerization of the crosslinking agent under the action of the catalyst can be avoided, the crosslinking process is added, so this method will also lead to an increase in equipment investment cost and operating cost.

[0007] The above prior art needs to spend time to pad and heat the crosslinking agent and the fiber multiple times during crosslinking, and requires a lot of equipment and steps. In view of this, a method for quickly preparing lyocell crosslinked staple fibers is proposed. Summary of the invention

[0008] The present invention aims to provide a method for rapidly preparing lyocell cross-linked staple fibers, simplify the cross-linking process, ensure that the staple fibers have anti-fibrillation properties, and reduce production energy consumption.

[0009] The technical solution of the present invention is as follows:

[0010] A method for rapidly preparing lyocell cross-linked staple fibers comprises the following steps:

[0011] S1, cutting the fiber filaments into short fibers;

[0012] S2, cross-linking agent solution preparation;

[0013] S3, placing the short fibers and the crosslinking agent solution into a reaction container at the same time, rotating, stirring and heating to perform a crosslinking reaction;

[0014] S4. After the cross-linking reaction is completed, water washing is performed to obtain Lyocell cross-linked short fibers with anti-fibrillation ability.

[0015] In this scheme, in the process of preparing cross-linked staple fibers, there is no need to fully contact the cross-linking agent solution with the target staple fibers in advance, nor is there a need for multiple immersion reactions. The target staple fibers and the prepared cross-linking agent solution are directly placed in a reaction container, and the cross-linking reaction can be completed after a certain period of rotation, stirring and heating. After subsequent water washing, lyocell staple fibers with good anti-fibrillation properties can be obtained, which is efficient and quick.

[0016] Preferably, in step S1, the length of the short fibers after cutting is 38 mm to 42 mm.

[0017] In order to select the appropriate concentration of crosslinking agent solution to ensure that the fiber can fully crosslink,

[0018] Preferably, in step S2, the crosslinking agent solution contains a crosslinking agent, a salt agent and an alkali agent, wherein the mass of the crosslinking agent is 1 / 100 to 1 / 10 of the mass of the staple fiber; the mass of the salt agent is 1 / 100 to 1 / 5 of the mass of the staple fiber; and the mass of the alkali agent is 1 / 100 to 1 / 5 of the mass of the fiber.

[0019] In this scheme, the alkali agent provides an alkaline environment to fully swell the fiber and increase the activity of the hydroxyl groups in the cellulose fiber. The salt agent can reduce the charge resistance between the crosslinking agent and the fiber, thereby improving the reaction efficiency of the crosslinking agent. The concentrations of the crosslinking agent, salt agent, and alkali agent vary with the amount of fiber added. The optimal ratio of the crosslinking agent is 1wt% of the fiber mass. If it is lower than this ratio, experiments show that the crosslinking effect will deteriorate; if it is higher than this ratio, it will not affect the crosslinking effect, but due to excessive crosslinking agent, it will cause a waste of resources.

[0020] Preferably, the amount of short fibers added in step S3 is 1 wt% to 20 wt% of the mass of the cross-linking agent solution.

[0021] In this scheme, the optimal addition ratio is 10wt%. A lower amount of short fiber added will not have any adverse effects, but will only reduce production efficiency. However, adding too much short fiber will cause the fluidity of the entire system to deteriorate after the fiber absorbs water, which is not conducive to the dispersion of the fiber in the cross-linking agent solution. The cross-linking agent solution is not evenly impregnated, resulting in a poor cross-linking effect.

[0022] Preferably, the rotation speed of the reaction container in step S3 is 0 to 100 rpm / s.

[0023] In this scheme, the short fibers and the crosslinking agent in the reaction container can fully contact and react by rotating and stirring, and continuous stirring can prevent the by-products produced by the reaction from hindering the contact between the short fibers and the crosslinking agent, effectively improving the rate and effect of the crosslinking reaction.

[0024] Appropriate heating can increase the reaction rate of the cross-linking reaction. In order to obtain the optimal heating temperature, the cross-linking reaction is carried out at different temperatures and the results are observed.

[0025] Preferably, the heating temperature in step S3 is 80-120° C., and the heating reaction time is 10-30 min.

[0026] In this scheme, the optimal heating range is 80-100°C. Experiments have shown that the cross-linking reaction takes a long time at low temperatures and a short time at high temperatures. If the temperature is lower than 80°C, the reaction efficiency of the cross-linking agent will be significantly reduced, resulting in poor cross-linking effect and poor fiber anti-fibrillation performance. However, when the temperature is higher than 100°C, the improvement in cross-linking reaction efficiency tends to be slow, which will result in an increase in energy consumption.

[0027] Preferably, in step S4, the cross-linking reaction wastewater needs to be discharged from the reaction container and then added with deionized water for washing with rotation and stirring.

[0028] Preferably, the water washing times are 1 to 3 times, and the water washing temperature is 40 to 50°C.

[0029] Preferably, the cross-linking agent is 1,3,5-triacryloylhexahydro-1,3,5-triazine, the alkali agent is Na2CO3, and the salt agent is Na2SO4.

[0030] Preferably, in step S3, the short fibers and the cross-linking agent solution are first mixed with each other to form a porridge-like fluid and then placed into the reaction container.

[0031] In this solution, the short fibers and the cross-linking agent solution are first mixed with each other, so that the short fibers can more easily enter the reaction container for reaction when the reaction container has only one feeding port.

[0032] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0033] In the present invention, the short fibers and the crosslinking agent solution are put into a reaction container together for a crosslinking reaction. The reaction container is continuously rotated, stirred and heated during the crosslinking reaction, and impregnation, heating crosslinking and water washing can all be carried out in one reaction container. There is no need to perform multiple impregnation and rolling during the crosslinking process as in the prior art, and there is no need to move the short fibers to a heating device for heating after impregnation, thereby avoiding the loss of the crosslinking agent. The crosslinking agent always reacts with the fibers before being discharged, thereby fully improving the utilization rate of the crosslinking agent. At the same time, compared with the prior art process, the present invention can use a lower temperature and a shorter time for heating, and optimizes and reduces the equipment and preparation steps used, effectively reducing the equipment cost and equipment energy consumption, and can efficiently and quickly prepare lyocell short fibers with good anti-fibrillation performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the drawings described below are only some embodiments. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the accompanying drawings:

[0035] Figure 1 It is a process flow chart of the present invention;

[0036] Figure 2 It is the detection observation diagram of each embodiment of the present invention and comparative example.

[0037] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0038] In conjunction with the accompanying drawings, the technical solution of the present invention is clearly and completely described through the specific implementation methods of the embodiments of the present invention.

[0039] Embodiment 1:

[0040] S1. Cut the fiber filaments into short fibers with a length of 38 mm;

[0041] S2. A crosslinking agent solution is prepared by mixing 1 / 100 of the mass of the staple fiber (1,3,5-triacryloylhexahydro-1,3,5-triazine), 1 / 50 of the mass of the staple fiber (Na2SO4) and 1 / 50 of the mass of the staple fiber (Na2CO3);

[0042] S3. Add the short fibers and the crosslinking agent solution into the reaction container, and ensure that the amount of the short fibers added is 10wt% of the mass of the crosslinking agent solution. After the short fibers and the crosslinking agent solution are added into the reaction container, the reaction container is started to rotate and stir, the heating temperature of the reaction container is set to 80°C, the rotation speed of the reaction container is set to 50rpm / min, and the heating crosslinking reaction is carried out for 20min.

[0043] It should be noted that the container and the crosslinking agent solution are preheated before the short fibers and the crosslinking agent solution are added to the reaction container, so that the short fibers and the crosslinking agent solution can reach the heating temperature immediately after entering the reaction container.

[0044] S4. After the waste liquid in the reaction container is discharged, deionized water is added and the mixture is washed twice at 40° C. to obtain Lyocell cross-linked staple fibers.

[0045] After obtaining the Lyocell cross-linked staple fibers, a portion of them were taken as samples for anti-fibrillation performance testing. The test was conducted using an ultrasonic cell crusher (LICHEN, LC-JY92-IIN) and observed under a microscope. The fewer microfibers peeled off from the fiber surface, the stronger the anti-fibrillation ability of the fiber.

[0046] The specific method is:

[0047] A. Immerse the cross-linked short fiber sample in deionized water to obtain a dispersion with a bath ratio (fiber / deionized water) of 1 mg / mL. Then place the dispersion in an ice water bath at 0°C and perform ultrasonic treatment on the dispersion. Finally, take out the fiber and remove the surface moisture. The distance between the ultrasonic probe and the bottom of the dispersion is 10 mm, the ultrasonic power is 500 W, and the ultrasonic treatment time is 20 min.

[0048] B. Take several samples from the treated short fibers, place them on a clean glass slide, add glycerol to disperse the fiber samples, cover them with a glass slide, place them under a microscope with a digital camera attachment, and take pictures after adjusting the magnification to a clear level. Figure 2 As shown in (a), it can be seen that the short fibers prepared in this example are almost not fibrillated.

[0049] Embodiment 2:

[0050] S1. Cut the fiber filaments into short fibers with a length of 38 mm;

[0051] S2. A crosslinking agent solution was prepared by mixing 1 / 50 of the mass of the staple fiber (1,3,5-triacryloylhexahydro-1,3,5-triazine), 1 / 25 of the mass of the staple fiber (Na2SO4) and 1 / 25 of the mass of the staple fiber (Na2CO3);

[0052] S3. Add the short fibers and the crosslinking agent solution to the reaction container, and ensure that the amount of short fibers added is 10wt% of the mass of the crosslinking agent solution. After adding the short fibers and the crosslinking agent solution to the reaction container, start the reaction container to start rotating and stirring, set the heating temperature of the reaction container to 80°C, set the rotating stirring speed of the reaction container to 50rpm / min, and perform a heating crosslinking reaction for 20min. It should be noted that the container and the crosslinking agent solution are preheated before the short fibers and the crosslinking agent solution are added to the reaction container, and the short fibers and the crosslinking agent solution can reach the heating temperature immediately after entering the reaction container.

[0053] S4. After the waste liquid in the reaction container is discharged, deionized water is added and the mixture is washed twice at 40° C. to obtain Lyocell cross-linked staple fibers.

[0054] That is, compared with Example 1, the addition amount of the cross-linking agent, the alkali agent and the salt agent in this example is doubled;

[0055] After obtaining the Lyocell cross-linked staple fibers, a portion of them were taken as samples for anti-fibrillation performance testing. The test was conducted using an ultrasonic cell crusher (LICHEN, LC-JY92-IIN) and observed under a microscope. The fewer microfibrils peeled off from the fiber surface, the stronger the anti-fibrillation ability of the fiber. Figure 2 As shown in (b), it can be seen that the short fibers prepared in this example are almost not fibrillated.

[0056] Embodiment three:

[0057] S1. Cut the fiber filaments into short fibers with a length of 38 mm;

[0058] S2. A crosslinking agent solution is prepared by mixing 1 / 100 of the mass of the staple fiber (1,3,5-triacryloylhexahydro-1,3,5-triazine), 1 / 50 of the mass of the staple fiber (Na2SO4) and 1 / 50 of the mass of the staple fiber (Na2CO3);

[0059] S3. Add the short fibers and the crosslinking agent solution to the reaction container, and ensure that the amount of short fibers added is 10wt% of the mass of the crosslinking agent solution. After adding the short fibers and the crosslinking agent solution to the reaction container, start the reaction container to start rotating and stirring, set the heating temperature of the reaction container to 100°C, set the rotating stirring speed of the reaction container to 50rpm / min, and perform a heating crosslinking reaction for 10 minutes. It should be noted that the container and the crosslinking agent solution are preheated before the short fibers and the crosslinking agent solution are added to the reaction container, so that the short fibers and the crosslinking agent solution can reach the heating temperature immediately after entering the reaction container.

[0060] S4. After the waste liquid in the reaction container is discharged, deionized water is added and the mixture is washed twice at 40° C. to obtain Lyocell cross-linked staple fibers.

[0061] That is, compared with Example 1, the heating temperature of the present embodiment during the reaction was increased to 100°C and the reaction time was shortened to 10 minutes. After obtaining the Lyocell cross-linked short fibers, a portion was taken as a sample for anti-fibrillation performance test. The test was performed using an ultrasonic cell crusher (LICHEN, LC-JY92-IIN) and observed under a microscope. The fewer microfibrils peeled off from the fiber surface, the stronger the anti-fibrillation ability of the fiber. The test observation results are as follows: Figure 2 As shown in (c), it can be seen that the short fibers prepared in this example are almost not fibrillated.

[0062] The lyocell cross-linked staple fibers prepared in the above examples all have good anti-fibrillation properties.

[0063] Comparative Example 1:

[0064] Compared with Example 1, the heating temperature in the cross-linking reaction process of this comparative example is set to 60° C., and the other process steps and the equipment used are consistent with Example 1. Finally, Lyocell cross-linked staple fibers are obtained.

[0065] The cross-linked short fibers of the comparative example were also tested for anti-fibrillation performance. The results obtained are as follows Figure 2 As shown in (d), it can be seen that a small amount of fibrils are peeled off from the short fibers prepared in this comparative example.

[0066] Comparative Example 2:

[0067] Compared with Example 1, the addition amount of the crosslinking agent, the alkali agent and the salt agent in this comparative example is reduced by half, that is, 1 / 200 of the mass of the staple fiber crosslinking agent (1,3,5-triacryloylhexahydro-1,3,5-triazine), 1 / 100 of the mass of the staple fiber salt agent (Na2SO4) and 1 / 100 of the mass of the staple fiber alkali agent (Na2CO3) are mixed to prepare a crosslinking agent solution. The other process steps and the equipment used are consistent with those in Example 1, and are not repeated here. Finally, Lyocell crosslinked staple fibers are obtained.

[0068] The cross-linked short fibers of the comparative example were also tested for anti-fibrillation performance. The results obtained from the test observation are as follows: Figure 2 As shown in (e), it can be seen that a small amount of fibrils are also peeled off from the short fibers prepared in this comparative example.

[0069] Comparative Example 3:

[0070] This comparative example uses the existing process to prepare cross-linked staple fibers, that is, the lyocell fiber filament bundle is immersed in a cross-linking agent solution at 80°C (the composition and concentration of the cross-linking agent solution are the same as those in Example 1) for 1 minute, the immersed filament bundle is centrifuged for dehydration, and then a high-temperature cross-linking reaction at 125°C is carried out in a heating device for 20 minutes, and finally two water washes at 40°C are carried out. After washing and cutting, Lyocell cross-linked staple fibers are obtained. The cross-linked staple fibers of this comparative example are tested for anti-fibrillation performance. The test results are as follows: Figure 2 As shown in (f), it can be seen that a small amount of original fibers are also peeled off from the short fibers prepared in this comparative example.

[0071] Comparative Example 4:

[0072] In this comparative example, no cross-linking reaction was performed, and the short fibers after being cut were directly tested by an ultrasonic cell crusher (LICHEN, LC-JY92-IIN). The test results are shown in FIG. Figure 2 (g) as shown.

[0073] Result analysis:

[0074] (1) By comparing and analyzing the results of Example 1, Example 2, Comparative Example 2 and Comparative Example 4, it can be seen that the concentration of the crosslinking agent has a great influence on the crosslinking process of the present patent. When the amount of the crosslinking agent added is greater than or equal to 1 / 100 of the fiber mass (Example 1 and Example 2), the crosslinked fiber has excellent anti-fibrillation performance compared with the uncrosslinked fiber (Comparative Example 4) while ensuring that other crosslinking processes are the same; when the amount of the crosslinking agent added is less than 1 / 100 of the fiber mass (Comparative Example 2), the anti-fibrillation performance of the crosslinked fiber will decrease. After ultrasonic treatment, a small amount of fibrils will be peeled off from the fiber, but it is still better than the anti-fibrillation performance of the uncrosslinked fiber (Comparative Example 4).

[0075] (2) By comparing and analyzing the results of Example 1, Example 3 and Comparative Example 1, it can be seen that the heating reaction temperature during the cross-linking process has a great influence on the cross-linking process of this patent. Under the condition that other cross-linking processes are the same, the cross-linked fiber prepared at a heating reaction temperature of 80°C (Example 1) has better anti-fibrillation performance than the cross-linked fiber prepared at a heating reaction temperature of 60°C (Comparative Example 1). Moreover, when the heating reaction temperature is increased to 100°C, the heating reaction time can be shortened to 10 minutes (Example 3), and the cross-linked fiber can also achieve the same anti-fibrillation level as the heating reaction temperature of 80°C and the heating reaction time of 20 minutes (Example 1).

[0076] (3) By comparing and analyzing the results of Example 1, Example 2, Example 3 and Comparative Example 3, it can be seen that the cross-linked staple fibers prepared by the process of the present invention (Example 1, Example 2 and Example 3) are better than the cross-linked staple fibers prepared by the cross-linking process of the prior art (Comparative Example 3). At the same time, Comparative Example 3 uses the existing process technology, which requires multiple steps of soaking, dehydration, heating reaction, and then washing and cutting. The process of the present invention only requires the prepared cross-linking agent solution and the staple fibers to be placed in a reaction container together with heating and rotating stirring. After washing, cross-linked staple fibers with good anti-fibrillation performance can be obtained, which greatly simplifies the process flow and also makes the cross-linked staple fibers have better anti-fibrillation performance; and the optimal temperature and the longest time used by the process of the present invention are less than or equal to the process of the prior art, which also reflects the advantage of the present invention in reducing production energy consumption; finally, the cross-linking agent solution of the present invention always maintains reaction contact with the staple fibers from the time of adding to the container to the time of discharging from the container, so there is no need to worry about the unnecessary loss and waste of the cross-linking agent, and the utilization rate of the cross-linking agent can be fully improved.

[0077] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for rapidly preparing lyocell cross-linked staple fibers, characterized in that: Included steps S1, cutting the fiber filaments into short fibers; S2, cross-linking agent solution preparation; S3, placing the short fibers and the crosslinking agent solution into a reaction container, rotating, stirring and heating to perform a crosslinking reaction; S4. After the cross-linking reaction is completed, water washing is performed to obtain Lyocell cross-linked short fibers with anti-fibrillation ability.

2. The method for rapidly preparing lyocell cross-linked staple fibers according to claim 1, characterized in that: In the step S1, the length of the short fibers after cutting is 38 mm to 42 mm.

3. A method for rapidly preparing lyocell cross-linked staple fibers according to claim 1 or 2, characterized in that: In step S2, the crosslinking agent solution contains a crosslinking agent, a salt agent and an alkali agent, wherein the mass of the crosslinking agent is 1 / 100 to 1 / 10 of the mass of the short fiber; the mass of the salt agent is 1 / 100 to 1 / 5 of the mass of the short fiber; and the mass of the alkali agent is 1 / 100 to 1 / 5 of the mass of the fiber.

4. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 1 to 3, characterized in that: The amount of short fibers added in step S3 is 1 wt% to 20 wt% of the crosslinking agent solution.

5. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 1 to 4, characterized in that: In step S3, the reaction container is rotated and stirred at a speed of 0 to 100 rpm / s.

6. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 1 to 5, characterized in that: The heating temperature in step S3 is 80-120° C., and the heating reaction time is 10-30 min.

7. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 1 to 6, characterized in that: In the step S4, the cross-linking reaction wastewater needs to be discharged from the reaction container and then added with deionized water for washing by rotation and stirring.

8. The method for rapidly preparing lyocell cross-linked staple fibers according to claim 7, characterized in that: The water washing times are 1 to 3 times, and the water washing temperature is 40 to 50°C.

9. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 3 to 7, characterized in that: The cross-linking agent is 1,3,5-triacryloylhexahydro-1,3,5-triazine, the alkali agent is Na2CO3, and the salt agent is Na2SO4.

10. A method for rapidly preparing lyocell cross-linked staple fibers according to any one of claims 1 to 9, characterized in that: In the step S3, the short fibers and the crosslinking agent solution are first mixed with each other to form a porridge-like fluid and then put into the reaction container.