Instrument for detecting mortar joint mortar strength through scratches and detection method
By designing a scratch detection instrument and using a telescopic cylinder and a diamond cutter head to score the mortar, the problem of detecting the strength of old building mortar in the existing technology has been solved, and convenient and accurate low-strength mortar detection has been achieved, which is suitable for old buildings. Mortar strength assessment for construction.
Patent Information
- Application Number
- CN202410752412.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
When the existing technology detects the strength of old building mortar, the local damage detection method has low acceptance. The non-damage detection method limits the minimum strength of the mortar, and the penetration method detection data is highly discrete and time-consuming, making it difficult to effectively detect low strength. mortar.
An instrument is designed for scratch detection of the strength of mortar joints. By setting up a telescopic cylinder and a diamond cutter head, the mortar can be scored. It is combined with a ball screw to drive the diamond cutter head to move, calculate the strength of the mortar, and apply a constant force. to achieve accurate detection.
It realizes the convenient and accurate detection of low-strength mortar, simplifies the operation, reduces the detection cost, and the detection results are representative, and is suitable for the evaluation of mortar strength of old buildings.
Smart Images

Figure CN118746481A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of detecting mortar strength by a scratch method, and specifically relates to an instrument and a detection method for detecting mortar strength of mortar joints by a scratch method. Background Art
[0002] Due to the rapid development of urbanization, most old buildings are facing reinforcement and renovation. Most of the old buildings are masonry structures, and the strength of their masonry mortar will directly affect the bearing capacity and earthquake safety of the house. Therefore, the standard test of mortar strength will be particularly important. At present, the local damage detection method (such as in-situ axial compression method, flat top method, in-situ single shear method, in-situ double shear method, etc.) recommended by the specification has low acceptance by the client and is generally not adopted. The mortar rebound method and point load method in the non-destructive detection method limit the minimum strength of the mortar to 2MPa, while the actual mortar strength of old buildings is generally low (0.4-7.5MPa). The above methods have their limitations; although the penetration method is not subject to the minimum strength limit, the detection data is highly discrete in the actual detection process, and the on-site operation is relatively time-consuming and labor-intensive.
[0003] Based on the above points, it is necessary to propose an instrument and method that is non-destructive, portable, low-priced, simple and quick to operate, and can detect low-strength grade mortar on site. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an instrument for scratching the strength of mortar joints in view of the shortcomings of the above-mentioned prior art. The instrument is provided with a telescopic cylinder and a metal rod to realize the extension and retraction of the metal rod, and a diamond bit is installed at the end of the metal rod, so that the diamond bit can be inserted into the mortar joints when the metal rod is extended, and a ball screw is provided to drive the telescopic cylinder to move, thereby driving the diamond bit inserted into the mortar joints to move, thereby realizing the scratching of the mortar joints, leaving scratches on the mortar joints, and calculating the strength of the mortar joints according to the scratches.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: an instrument for scratch detection of mortar strength in mortar joints, characterized in that the instrument includes a body, a ball screw is arranged inside the body, a telescopic cylinder is arranged on the nut of the ball screw, the telescopic movement direction of the telescopic cylinder is perpendicular to the axial direction of the screw of the ball screw, a metal rod is connected to the output end of the telescopic cylinder, a diamond bit is arranged on the end of the metal rod away from the telescopic cylinder, and a long groove for the diamond bit to extend out is opened on the body.
[0006] The above-mentioned instrument for scratch testing the mortar strength of mortar joints is characterized in that two support blocks are arranged in parallel on both sides of the long groove on the outer surface of the body, and the gap between the two support blocks is greater than the width of the mortar joint.
[0007] The above-mentioned instrument for scratch testing the strength of mortar joints is characterized in that a reset button for restoring the telescopic cylinder to a retracted state is provided on the body.
[0008] The above-mentioned instrument for detecting the strength of mortar joints by scratching is characterized in that a display screen for displaying the extended length of the metal rod is provided on the body.
[0009] The above-mentioned instrument for scratch testing the strength of mortar joints is characterized in that the diameter of the metal rod is 6mm to 10mm, the diamond bit is a conical structure, the bottom diameter of the conical structure is the same as the diameter of the metal rod, and the height of the conical structure is 1mm to 2mm.
[0010] In addition, the present invention also provides a method for detecting the strength of mortar joints by scratching, characterized in that the method comprises the following steps:
[0011] Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the wall surface, and then grind the mortar joints to make them smooth to obtain the wall to be tested; the number of the walls to be tested is multiple;
[0012] Step 2: Position selection: evenly select multiple test mortar joints on the wall to be tested obtained in step 1, and select multiple positions on each test mortar joint;
[0013] Step 3, instrument layout: place the two support blocks of the instrument close to the upper and lower brick surfaces of any mortar joint selected in step 2, so that the diamond bit is placed at the position of the mortar joint, and obtain the positioning instrument;
[0014] Step 4: Zeroing the instrument: Open the telescopic cylinder in the positioning instrument obtained in step 3, make the diamond bit close to the ash seam, and then adjust the extension length of the metal rod to zero to obtain a zeroing instrument;
[0015] Step 5, detection and measurement: Open the telescopic cylinder in the zeroing instrument obtained in step 4, so that the diamond bit extends into the mortar joint with a constant force, and then open the ball screw to make the diamond bit scratch on the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5 to scratch all the measuring positions of each wall to be tested to obtain the maximum scratch depth value of all the measuring positions;
[0016] Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately to obtain the representative scratch depth value of each wall, then perform regression calculation on the obtained representative scratch depth value of each wall to obtain the converted value of mortar compressive strength of mortar joints of each wall, then perform comprehensive calculation on all the converted values of mortar compressive strength of mortar joints of each wall to obtain the mortar joint strength of the batch of walls.
[0017] The present invention enables the diamond bit to extend into the mortar joint by applying a constant force, so that the instrument can do work on the mortar. The surface hardness of the mortar can be used to reflect the strength of the mortar. Therefore, through the two steps of insertion and scratching, the work done is converted into the depth of the scratch, which is used to reflect the surface hardness of the mortar and further reflect the strength of the mortar.
[0018] The above method is characterized in that the wall to be tested in step 1 is 5 to 10 faces, the test mortar joints in step 2 are 10 to 12, 1 to 2 positions are selected on each test mortar joint, and the horizontal distance of adjacent positions is greater than 240 mm. The mortar joint mortar strength test in the present invention is mainly carried out on a building, and a building is divided into inspection batches according to the number of floors. Multiple walls are selected on each floor as an inspection batch, and multiple mortar joints should be selected for each wall. Multiple positions are tested for each mortar joint, and the position arrangement should be evenly distributed on the horizontal mortar joints to obtain the mortar joint mortar strength of the building; the present invention increases the test amount by controlling the number of faces of the wall to be tested, the number of mortar joints and the number of positions, and ensures that the test results are representative. The horizontal distance of adjacent positions is controlled because the process of masonry mortar will have a situation where the local mortar mixing is poor. If the local mortar mixing is poor, the strength will be low. At the same time, the test positions on both sides of the adjacent sides are selected in this area, which may cause the final test result to be affected by the low local mortar strength and deviate.
[0019] It should be noted that when two measurement positions are selected on a gray seam, the larger of the maximum depths of the scratches obtained from the two measurement positions is used as the scratch depth of the gray seam.
[0020] The above method is characterized in that the constant force in step five is 390N to 410N, and the length of the scratch is 80mm to 120mm. In the present invention, the minimum strength of the mortar joint is generally 2MPa, while the strength of the mortar in old buildings is generally low, 0.4MPa to 7.5MPa. The present invention controls the magnitude of the constant force to leave uniform scratches on the mortar joint, and better controls the depth of the scratches within a certain range, which is convenient for instrument measurement. By controlling the length of the scratches, it is convenient to measure the depth value, and the length can more stably reflect the strength of the mortar.
[0021] The above method is characterized in that the process of separate calculation in step 6 is: remove a maximum value and a minimum value of the maximum scratch depth values of all measured positions on a wall, take the average value of the remaining maximum scratch depth values, and obtain the representative value of the scratch depth of the wall, repeat the above process to obtain the representative value of the scratch depth of each wall; the process of regression calculation is: substitute the representative value of the scratch depth of a wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d is the converted value of the compressive strength of the mortar joints; the comprehensive calculation process is: remove a maximum value and a minimum value from the converted values of the compressive strength of the mortar joints of all walls, and average the remaining converted values of the compressive strength of the mortar joints to obtain the mortar strength of the batch of walls. In the present invention, in the separate calculation, remove a maximum value and a minimum value from the maximum scratch depth values of all measured positions on a wall, and average the remaining maximum scratch depth values to obtain the representative value of the scratch depth of the wall, wherein the maximum value and the minimum value are removed to ensure the accuracy of the mortar strength; in the regression calculation, f is used d =186.0815d m -2.0740 The calculation is performed, and the formula is obtained by curve fitting of a large amount of experimental data. Specifically, mortar test blocks with different mix ratios are designed, and the strength grades are M1, M2, M2.5, M5, M7.5, and M10, totaling 6 strength grades. 144 cubic test blocks with a side length of 70.7 mm are made for each strength grade. After natural curing to the age, the four sides of the mortar test blocks are scratched by the instrument of the present invention, and the average value of the scratch depth is recorded. After the recording is completed, the mortar test blocks are subjected to a compressive strength test by a testing machine, and the compressive strength values of different mortar test blocks are recorded. According to the compressive strength corresponding to different scratch depths of each test block, the formula f is finally fitted through data processing and analysis. d =186.0815d m -2.0740 , which also ensures the accuracy of the mortar joint strength; in the comprehensive calculation, the mortar joint compressive strength conversion values of all walls are removed by removing a maximum value and a minimum value, and the remaining mortar joint compressive strength conversion values are averaged to obtain the mortar joint strength of the batch of walls, which ensures the accuracy of the mortar joint strength.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. The present invention realizes the extension and retraction of the metal rod by arranging a telescopic cylinder and installing a metal rod. By installing a diamond cutter head at the end of the metal rod, the diamond cutter head is conveniently inserted into the mortar joint when the metal rod is extended. A ball screw is arranged to drive the telescopic cylinder to move, thereby driving the diamond cutter head inserted into the mortar joint to move, thereby achieving the scoring of the mortar joint, leaving scratches on the mortar joint, and calculating the strength of the mortar joint based on the scratches.
[0024] 2. The present invention applies a constant force to make the diamond bit extend into the mortar joint, so that the instrument can do work on the mortar. The surface hardness of the mortar can be used to reflect the strength of the mortar. Therefore, through the two steps of insertion and scratching, the work done is converted into the depth of the scratch, which is used to reflect the surface hardness of the mortar and further reflect the strength of the mortar.
[0025] 3. The present invention converts the scratch depth value into the mortar joint strength through separate calculation, regression calculation and comprehensive calculation, and obtains the mortar joint strength through the scratch depth, which has the advantages of simple calculation and high accuracy.
[0026] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure of an instrument for detecting the strength of mortar joints by scratching according to the present invention.
[0028] Figure 2 The invention discloses a schematic diagram of the connection relationship between a ball screw, a telescopic cylinder and a metal rod in an instrument for detecting the strength of mortar joints by scratching.
[0029] Description of reference numerals:
[0030] 1—machine body; 2—ball screw; 3—nut;
[0031] 4—screw rod; 5—telescopic cylinder; 6—metal rod;
[0032] 7—diamond bit; 8—long slot; 9—support block;
[0033] 10—Reset button; 11—Display screen. DETAILED DESCRIPTION
[0034] An instrument for detecting the strength of mortar joints by scratching according to the present invention is described in detail through Example 1.
[0035] Example 1
[0036] like Figure 1 and Figure 2As shown, the instrument for scratch testing the mortar strength of mortar joints of this embodiment comprises a body 1, a ball screw 2 is arranged inside the body 1, a telescopic cylinder 5 is arranged on the nut 3 of the ball screw 2, the telescopic movement direction of the telescopic cylinder 5 is perpendicular to the axial direction of the screw 4 of the ball screw 2, a metal rod 6 is connected to the output end of the telescopic cylinder 5, a diamond bit 7 is arranged on the end of the metal rod 6 away from the telescopic cylinder 5, and a long slot 8 for the diamond bit 7 to extend out is opened on the body 1.
[0037] It should be noted that, by providing the machine body 1, that is, providing a shell for mounting components such as the ball screw 2 and the telescopic cylinder 5 inside, the long slot 8 is provided to facilitate the extension of the metal rod 6 and the diamond bit 7.
[0038] It should be noted that by providing a telescopic cylinder 5 and installing a metal rod 6, the extension and retraction of the metal rod 6 can be achieved. By installing a diamond cutter head 7 at the end of the metal rod 6, the diamond cutter head 7 can be easily inserted into the mortar joint when the metal rod 6 is extended. By providing a ball screw 2 to drive the telescopic cylinder 5 to move, the diamond cutter head 7 inserted into the mortar joint can be driven to move, thereby achieving the scoring of the mortar joint, leaving scratches on the mortar joint, and calculating the strength of the mortar joint based on the scratches.
[0039] like Figure 1 and Figure 2 As shown, in this embodiment, two support blocks 9 are arranged in parallel on both sides of the long groove 8 on the outer surface of the body 1, and the gap between the two support blocks 9 is greater than the width of the mortar joint. By setting two support blocks 9, the instrument can be better pressed against the wall, and the metal rod 6 can be easily extended and retracted.
[0040] It should be noted that the length of the support block 9 is 100 mm to 200 mm, preferably 100 mm, 150 mm and 200 mm, the width of the support block 9 is 10 mm to 30 mm, preferably 10 mm, 20 mm and 30 mm, and the height of the support block 9 is 10 mm to 20 mm, preferably 10 mm, 15 mm and 20 mm. By controlling the size of the two support blocks 9, the instrument can be better pressed against the wall.
[0041] like Figure 1 As shown, in this embodiment, a reset button 10 for restoring the telescopic cylinder 5 to a retracted state is provided on the machine body 1. By providing the reset button 10, the telescopic cylinder 5 is restored to a retracted state, so that the instrument can be restored to an initial state. In the initial state, the metal rod 6 and the diamond bit 7 are in a retracted state, so that it is convenient to leave scratches on the mortar joint later.
[0042] like Figure 1As shown, in this embodiment, a display screen 11 for displaying the extension length of the metal rod 6 is provided on the machine body 1. By setting the display screen 11 to display the extension length of the metal rod 6, that is, to display the depth of the diamond bit 7 at the front end of the metal rod 6 inserted into the mortar joint, the depth of the scratch obtained in the mortar joint can be obtained.
[0043] It should be noted that the body 1 is also provided with a component that cooperates with the display screen 11 and adjusts the extended length of the metal rod 6 to zero. Because when the telescopic cylinder 5 is in the initial state, that is, the contracted state, the diamond cutter head 7 on the metal rod 6 is at a certain distance from the mortar joint mortar. At this time, the metal rod 6 needs to be extended to make the diamond cutter head 7 rest against the mortar joint mortar. At this time, the metal rod 6 has been extended to a certain length, but this length is meaningless for the mortar joint mortar strength test. Therefore, when the diamond cutter head 7 rests on the mortar joint mortar, the extended length of the metal rod 6 is adjusted to zero, so as to obtain the depth of the diamond cutter head 7 inserted into the mortar joint mortar, thereby obtaining the depth of the scratch on the mortar joint mortar.
[0044] In this embodiment, the diameter of the metal rod 6 is 6 mm to 10 mm, and the diamond bit 7 is a conical structure, the bottom diameter of the conical structure is the same as the diameter of the metal rod 6, and the height of the conical structure is 1 mm to 2 mm. By controlling the shape and size of the metal rod 6 and the diamond bit 7, it is convenient for the diamond bit 7 to obtain appropriate scratches in the mortar joint.
[0045] The method for detecting the strength of mortar joints by scratching of the present invention is described in detail through Examples 2 to 5.
[0046] Example 2
[0047] This embodiment includes the following steps:
[0048] Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the surface of 5 walls, and then grind the mortar joints to make them smooth to obtain 5 walls to be tested;
[0049] Step 2, location selection: 12 test mortar joints are evenly selected on the 5 test walls obtained in step 1, and 1 to 2 locations are selected on each test mortar joint, and the horizontal distance between adjacent locations is greater than 240 mm;
[0050] Step 3, instrument layout: place the two support blocks 9 of the instrument close to the upper and lower brick surfaces of any one of the mortar joints selected in step 2, so that the diamond bit 7 is placed at the position of the mortar joint to obtain a positioning instrument;
[0051] Step 4: Zeroing the instrument: Open the telescopic cylinder 5 in the positioning instrument obtained in step 3, make the diamond bit 7 close to the ash seam, and then adjust the extension length of the metal rod 6 to zero to obtain a zeroing instrument;
[0052] Step 5, detection and measurement: Open the telescopic cylinder 5 in the zeroing instrument obtained in step 4, so that the diamond bit 7 extends into the mortar joint with a constant force of 400N, and then open the ball screw 2, so that the diamond bit 7 scratches 100mm on the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5, scratch all the measured positions of each wall to be detected, and obtain the maximum scratch depth value of all the measured positions;
[0053] Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately, remove the maximum value and the minimum value of the maximum scratch depth values of all measured positions on one wall, and take the average value of the remaining maximum scratch depth values to obtain the representative scratch depth value of the wall. Repeat the above process to obtain the representative scratch depth value of each wall, and then perform regression calculation on the obtained representative scratch depth value of each wall, and substitute the representative scratch depth value of one wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d The mortar joint compressive strength conversion value is obtained, and then the mortar joint compressive strength conversion values of all walls are comprehensively calculated. The mortar joint compressive strength conversion values of all walls are removed with a maximum value and a minimum value, and the remaining mortar joint compressive strength conversion values are averaged to obtain the mortar joint strength of this batch of walls. The test and calculation results are shown in Table 1.
[0054] Table 1
[0055]
[0056]
[0057]
[0058] After calculation, the mortar strength of the mortar joints of the batch of walls in this embodiment is 3.09 MPa.
[0059] Example 3
[0060] This embodiment includes the following steps:
[0061] Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the surface of the 7 walls, and then grind the mortar joints to make them smooth, and obtain 7 walls to be tested;
[0062] Step 2, location selection: 11 test mortar joints are evenly selected on the 7 test walls obtained in step 1, and 1 to 2 locations are selected on each test mortar joint, and the horizontal distance between adjacent locations is greater than 240 mm;
[0063] Step 3, instrument layout: place the two support blocks 9 of the instrument close to the upper and lower brick surfaces of any one of the mortar joints selected in step 2, so that the diamond bit 7 is placed at the position of the mortar joint to obtain a positioning instrument;
[0064] Step 4: Zeroing the instrument: Open the telescopic cylinder 5 in the positioning instrument obtained in step 3, make the diamond bit 7 close to the ash seam, and then adjust the extension length of the metal rod 6 to zero to obtain a zeroing instrument;
[0065] Step 5, detection and measurement: Open the telescopic cylinder 5 in the zeroing instrument obtained in step 4, so that the diamond bit 7 extends into the mortar joint with a constant force of 410N, and then open the ball screw 2, so that the diamond bit 7 scratches 80mm on the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5, scratch all the measured positions of each wall to be tested, and obtain the maximum scratch depth value of all the measured positions;
[0066] Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately, remove the maximum value and the minimum value of the maximum scratch depth values of all measured positions on one wall, and take the average value of the remaining maximum scratch depth values to obtain the representative scratch depth value of the wall. Repeat the above process to obtain the representative scratch depth value of each wall, and then perform regression calculation on the obtained representative scratch depth value of each wall, and substitute the representative scratch depth value of one wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d The mortar joint compressive strength conversion value is obtained, and then the mortar joint compressive strength conversion values of all walls are comprehensively calculated. The mortar joint compressive strength conversion values of all walls are removed with a maximum value and a minimum value, and the remaining mortar joint compressive strength conversion values are averaged to obtain the mortar joint strength of this batch of walls. The test and calculation results are shown in Table 2.
[0067] Table 2
[0068]
[0069]
[0070]
[0071] After calculation, the mortar strength of the mortar joints of the batch of walls in this embodiment is 2.75MPa.
[0072] Example 4
[0073] This embodiment includes the following steps:
[0074] Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the surface of 8 walls, and then grind the mortar joints to make them smooth, and obtain 8 walls to be tested;
[0075] Step 2, location selection: 10 test mortar joints are evenly selected on the 8 test walls obtained in step 1, and 1 to 2 locations are selected on each test mortar joint, and the horizontal distance between adjacent locations is greater than 240 mm;
[0076] Step 3, instrument layout: place the two support blocks 9 of the instrument close to the upper and lower brick surfaces of any one of the mortar joints selected in step 2, so that the diamond bit 7 is placed at the position of the mortar joint to obtain a positioning instrument;
[0077] Step 4: Zeroing the instrument: Open the telescopic cylinder 5 in the positioning instrument obtained in step 3, make the diamond bit 7 close to the ash seam, and then adjust the extension length of the metal rod 6 to zero to obtain a zeroing instrument;
[0078] Step 5, detection and measurement: Open the telescopic cylinder 5 in the zeroing instrument obtained in step 4, so that the diamond bit 7 extends into the mortar joint with a constant force of 390N, and then open the ball screw 2, so that the diamond bit 7 scratches 120mm on the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5, scratch all the measured positions of each wall to be tested, and obtain the maximum scratch depth value of all the measured positions;
[0079] Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately, remove the maximum value and the minimum value of the maximum scratch depth values of all measured positions on one wall, and take the average value of the remaining maximum scratch depth values to obtain the representative scratch depth value of the wall. Repeat the above process to obtain the representative scratch depth value of each wall, and then perform regression calculation on the obtained representative scratch depth value of each wall, and substitute the representative scratch depth value of one wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d The mortar joint compressive strength conversion value is obtained, and then the mortar joint compressive strength conversion values of all walls are comprehensively calculated. The mortar joint compressive strength conversion values of all walls are removed with a maximum value and a minimum value, and the remaining mortar joint compressive strength conversion values are averaged to obtain the mortar joint strength of this batch of walls. The test and calculation results are shown in Table 3.
[0080] Table 3
[0081]
[0082]
[0083]
[0084] After calculation, the mortar strength of the mortar joints of the batch of walls in this embodiment is 2.23 MPa.
[0085] Example 5
[0086] This embodiment includes the following steps:
[0087] Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the surface of 10 walls, and then grind the mortar joints to make them smooth, and obtain 10 walls to be tested;
[0088] Step 2, location selection: 10 test mortar joints are evenly selected on the 10 walls to be tested obtained in step 1, and 1 to 2 locations are selected on each test mortar joint, and the horizontal distance between adjacent locations is greater than 240 mm;
[0089] Step 3, instrument layout: place the two support blocks 9 of the instrument close to the upper and lower brick surfaces of any one of the mortar joints selected in step 2, so that the diamond bit 7 is placed at the position of the mortar joint to obtain a positioning instrument;
[0090] Step 4: Zeroing the instrument: Open the telescopic cylinder 5 in the positioning instrument obtained in step 3, make the diamond bit 7 close to the ash seam, and then adjust the extension length of the metal rod 6 to zero to obtain a zeroing instrument;
[0091] Step 5, detection and measurement: Open the telescopic cylinder 5 in the zeroing instrument obtained in step 4, so that the diamond bit 7 extends into the mortar joint with a constant force of 405N, and then open the ball screw 2, so that the diamond bit 7 scratches 90mm on the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5, scratch all the measured positions of each wall to be tested, and obtain the maximum scratch depth value of all the measured positions;
[0092] Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately, remove the maximum value and the minimum value of the maximum scratch depth values of all measured positions on one wall, and take the average value of the remaining maximum scratch depth values to obtain the representative scratch depth value of the wall. Repeat the above process to obtain the representative scratch depth value of each wall, and then perform regression calculation on the obtained representative scratch depth value of each wall, and substitute the representative scratch depth value of one wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d The mortar joint compressive strength conversion value is obtained, and then the mortar joint compressive strength conversion values of all walls are comprehensively calculated, and the maximum value and the minimum value of the mortar joint compressive strength conversion values of all walls are removed. The remaining mortar joint compressive strength conversion values are averaged to obtain the mortar joint strength of this batch of walls.
[0093] After calculation, the mortar strength of the mortar joints of the batch of walls in this embodiment is 2.58 MPa.
[0094] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. An instrument for scratch testing the strength of mortar joints, characterized in that: The instrument comprises a body (1), wherein a ball screw (2) is arranged inside the body (1), a telescopic cylinder (5) is arranged on a nut (3) of the ball screw (2), the telescopic movement direction of the telescopic cylinder (5) is perpendicular to the axial direction of a screw rod (4) of the ball screw (2), a metal rod (6) is connected to the output end of the telescopic cylinder (5), a diamond cutter head (7) is arranged at one end of the metal rod (6) away from the telescopic cylinder (5), and a long slot (8) for the diamond cutter head (7) to extend is opened on the body (1).
2. The instrument for detecting the strength of mortar joints by scratching according to claim 1 is characterized in that: Two support blocks (9) are arranged in parallel on both sides of the long groove (8) on the outer surface of the machine body (1), and the gap between the two support blocks (9) is greater than the width of the mortar joint.
3. The instrument for detecting the strength of mortar joints by scratching according to claim 1 is characterized in that: The machine body (1) is provided with a reset button (10) for restoring the telescopic cylinder (5) to a retracted state.
4. The instrument for detecting the strength of mortar joints by scratching according to claim 1 is characterized in that: The machine body (1) is provided with a display screen (11) for displaying the extended length of the metal rod (6).
5. The instrument for detecting the strength of mortar joints by scratching according to claim 1 is characterized in that: The diameter of the metal rod (6) is 6 mm to 10 mm, the diamond bit (7) is a conical structure, the bottom diameter of the conical structure is the same as the diameter of the metal rod (6), and the height of the conical structure is 1 mm to 2 mm.
6. A method for scratch testing the strength of mortar joints using the instrument as claimed in any one of claims 1 to 5, characterized in that: The method comprises the following steps: Step 1: Remove the wall finishing layer: remove the finishing layer, paint layer, joint mortar, floating slurry and surface damage layer on the wall surface, and then grind the mortar joints to make them smooth to obtain the wall to be tested; the number of the walls to be tested is multiple; Step 2: Position selection: evenly select multiple test mortar joints on the wall to be tested obtained in step 1, and select multiple positions on each test mortar joint; Step 3, instrument layout: place the two support blocks (9) of the instrument close to the upper and lower brick surfaces of any one of the mortar joints selected in step 2, so that the diamond bit (7) is placed at the position of the mortar joint, and obtain a positioning instrument; Step 4, zeroing the instrument: Open the telescopic cylinder (5) in the positioning instrument obtained in step 3, make the diamond bit (7) close to the ash seam, and then adjust the extension length of the metal rod (6) to zero, so as to obtain a zeroing instrument; Step 5, detection and measurement: Open the telescopic cylinder (5) in the zeroing instrument obtained in step 4, so that the diamond bit (7) extends into the mortar joint with a constant force, and then open the ball screw (2) so that the diamond bit (7) scratches the mortar joint to obtain a scratch, and then detect the maximum depth of the scratch, and then repeat steps 3 to 5 to scratch all the measured positions of each wall to be detected to obtain the maximum scratch depth value of all the measured positions; Step 6. Calculation of mortar compressive strength: Calculate the maximum scratch depth values of all measured positions obtained in step 5 for each wall separately to obtain the representative scratch depth value of each wall, then perform regression calculation on the obtained representative scratch depth value of each wall to obtain the converted value of mortar compressive strength of mortar joints of each wall, then perform comprehensive calculation on all the converted values of mortar compressive strength of mortar joints of each wall to obtain the mortar joint strength of the batch of walls.
7. The method according to claim 6, characterized in that In step 1, there are 5 to 10 walls to be tested, and in step 2, there are 10 to 12 test joints. One to two measurement positions are selected on each test joint, and the horizontal distance between adjacent measurement positions is greater than 240 mm.
8. The method according to claim 6, characterized in that The constant force in step five is 390N to 410N, and the length of the engraving is 80mm to 120mm.
9. The method according to claim 6, characterized in that The process of separate calculation in step 6 is: take the maximum scratch depth values of all measured positions of a wall, remove the maximum value and the minimum value, take the average value of the remaining maximum scratch depth values, and obtain the representative value of the scratch depth of the wall, repeat the above process to obtain the representative value of the scratch depth of each wall; the process of regression calculation is: substitute the representative value of the scratch depth of a wall into the regression formula f d =186.0815d m -2.0740 Calculate and obtain the converted value of the mortar compressive strength of the wall joints. Repeat the above process to obtain the converted value of the mortar compressive strength of each wall joints, where d m is the representative value of the scratch depth, f d is the converted value of the compressive strength of the mortar joints; the comprehensive calculation process is: the converted values of the compressive strength of the mortar joints of all walls are removed from a maximum value and a minimum value, and the remaining converted values of the compressive strength of the mortar joints are averaged to obtain the mortar strength of the mortar joints of the batch of walls.