Three-dimensional layered zinc negative electrode and preparation method and application thereof

By treating the surface of pure zinc with an inorganic metal salt solution, a three-dimensional layered zinc anode with a uniform surface is prepared, which solves the problems of zinc dendrite growth and side reactions, realizes a 3D zinc anode with excellent cycle performance and safety, and improves battery storage capacity and energy density, and reduce preparation costs.

CN118748237AInactive Publication Date: 2024-10-08GUIZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410819647.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The commercialization of existing aqueous zinc-ion batteries is hindered by zinc dendrite growth and side reactions (such as hydrogen evolution reaction), and the common 3D pure zinc anode constructed by inorganic acid etching has problems of poor safety and poor reversibility.

Method used

Inorganic metal salt solution, especially ammonium persulfate solution, is dropped on the surface of pure zinc for standing, washing and drying to prepare a three-dimensional layered zinc anode with a uniform surface, changing the morphology of the zinc anode and increasing the surface area and active sites. points, lowering the nucleation energy barrier, increasing battery capacity and energy density, and enhancing mechanical stability through a 3D layered structure.

Benefits of technology

A 3D zinc anode with excellent cycle performance and safety has been achieved, which improves the storage capacity and energy density of the battery, slows down the battery capacity fading rate, reduces the electron and ion transmission path, enhances mechanical stability, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748237A_ABST
    Figure CN118748237A_ABST
Patent Text Reader

Abstract

The invention provides a three-dimensional layered zinc negative electrode and a preparation method and application thereof, and belongs to the technical field of aqueous zinc ion batteries. Pure zinc is treated by adopting an inorganic metal salt solution, the zinc negative electrode with a uniform 3D layered structure on the surface is obtained, the surface area of the zinc negative electrode is increased, more active sites are provided, and introduction of zinc-loving sites is beneficial to reduction of nucleation energy barriers and homogenization of Zn < 2 + > flux, so that the capacity and energy density of the battery are improved; meanwhile, a shorter electron and ion transmission path can be provided, and the interface resistance is reduced; and moreover, more effective nesting and releasing of zinc ions are facilitated, the storage capacity of the battery is improved, and the capacity fading speed of the battery is slowed down. In addition, the 3D layered structure is beneficial for improving the mechanical stability of the zinc negative electrode and reducing the problem of structural collapse caused by expansion and contraction of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous zinc ion batteries, and in particular relates to a three-dimensional layered zinc negative electrode and a preparation method and application thereof. Background Art

[0002] With the depletion of traditional fossil fuels and the increasing environmental pollution, the development and utilization of renewable energy (solar energy, geothermal energy, wind energy, etc.) has attracted great attention. Energy storage systems are expected to achieve large-scale application of renewable energy. Among many energy storage systems, the zinc anode in aqueous zinc-ion batteries has high safety, high theoretical specific capacity (820 mAh g -1 and 5585mAh cm -3 ), low redox potential (-0.76 V vs standard hydrogen electrode), low cost, abundant reserves, and environmental friendliness have attracted widespread attention. Unfortunately, the commercialization of aqueous Zn-ion batteries still faces inevitable obstacles due to the growth of Zn dendrites and side reactions such as hydrogen evolution reaction (HER) and corrosion.

[0003] In order to solve the above problems, researchers have proposed many strategies such as electrolyte optimization, three-dimensional zinc (3D) anode construction, zinc anode surface modification and separator modification. Among them, 3D pure zinc anode construction is one of the most effective methods to establish a stable electrode / electrolyte interface to inhibit zinc anode surface dendrite growth and side reactions.

[0004] The existing document “Chemically polished zinc metal electrode with a ridge-like structure for cycle-stable aqueous batteries” discloses that a 3D ridged zinc negative electrode is constructed by ultrasonically cleaning zinc foil with hydrochloric acid. This method can remove impurities on the surface of zinc foil, expose a large amount of active zinc on the surface of the zinc negative electrode, make the electric field on the electrode surface uniformly distributed, and induce uniform zinc deposition. The document “Microgroove-patterned Zn metalanode enables ultra-stable and low-overpotential Zn deposition for long-cycling aqueous batteries” discloses that a zinc negative electrode with a microgroove structure on the surface is prepared by etching the surface of zinc foil with low concentration hydrochloric acid, thereby achieving ultra-stable zinc deposition at extremely low overpotential. The document “A Theory-driven complementary interface effect for fast-kinetics and ultrastable Znmetal anodes in aqueous / solid electrolytes” discloses that the surface structure of the zinc metal negative electrode is directional etched by boric acid hydrothermal treatment, and a coordinated modulation dual interface strategy is constructed in one step as a new way to stabilize the zinc negative electrode. However, the above-mentioned etching method using common inorganic acids (such as hydrochloric acid, boric acid, etc.) to construct a 3D pure zinc negative electrode has the disadvantages of poor safety, high volatility, high corrosion, etc., and the constructed 3D pure zinc negative electrode has poor reversibility.

[0005] Therefore, there is an urgent need for a preparation method of a 3D zinc negative electrode with excellent cycle performance, safety and low cost to solve the above problems. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a three-dimensional layered zinc negative electrode and a preparation method and application thereof.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a three-dimensional layered zinc negative electrode, comprising the following steps:

[0009] An inorganic metal salt solution is dropped onto the pure zinc surface, and after standing, washing and drying, a three-dimensional layered zinc negative electrode is obtained.

[0010] Preferably, the inorganic metal salt in the inorganic metal salt solution is ammonium persulfate.

[0011] Preferably, the concentration of the inorganic metal salt solution is 0.05-3 mol / L.

[0012] Preferably, the concentration of the inorganic metal salt solution is 0.05-0.3 mol / L.

[0013] Preferably, the standing temperature is room temperature and the standing time is 1-9 minutes.

[0014] The present invention provides a three-dimensional layered zinc negative electrode prepared by the preparation method of the three-dimensional layered zinc negative electrode described in the above technical solution.

[0015] The present invention also provides an application of the three-dimensional layered zinc negative electrode described in the above technical solution, and assembles the above three-dimensional layered zinc negative electrode into a symmetrical battery, a hybrid supercapacitor or a full battery.

[0016] Preferably, the assembling of the three-dimensional layered zinc negative electrode into a symmetrical battery comprises the following steps: using the three-dimensional layered zinc negative electrode as the positive electrode and the negative electrode, respectively, and assembling them with a separator and an electrolyte into a symmetrical battery.

[0017] Preferably, the assembling of the three-dimensional layered zinc negative electrode into a hybrid supercapacitor or a full battery comprises the following steps: using the three-dimensional layered zinc as the negative electrode, and assembling it with the positive electrode, electrolyte and separator into a hybrid supercapacitor or a full battery.

[0018] Preferably, the separator is a glass fiber separator or a cellulose separator.

[0019] Compared with the prior art, the present invention has the following advantages and technical effects:

[0020] The present invention uses an inorganic metal salt solution to treat a pure zinc negative electrode, thereby changing the morphology of the zinc negative electrode and obtaining a zinc negative electrode with a uniform 3D layered structure on the surface, thereby effectively increasing the surface area of ​​the zinc negative electrode, providing more active sites, and helping to reduce the nucleation energy barrier. 2+ The flux is homogenized, thereby increasing the capacity and energy density of the battery; it can also provide a shorter electron and ion transmission path and reduce the interface resistance; it also helps to more effectively nest and release zinc ions, increase the storage capacity of the battery, and slow down the rate of battery capacity decay; and the 3D layered structure helps to improve the mechanical stability of the zinc negative electrode and reduce the structural collapse problem caused by electrode expansion and contraction. In addition, the preparation method provided by the present invention is simple, safe, and low-cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0022] Figure 1 A schematic diagram of the process of preparing a three-dimensional layered zinc negative electrode according to Examples 1-8 of the present invention;

[0023] Figure 2 The scanning electron microscope images are of the pure zinc negative electrode in step 1) of Example 5 and the L-Zn-0.05-3 negative electrode prepared in Example 5;

[0024] Figure 3 The X-ray diffraction patterns of the pure zinc negative electrode in step 1) of Example 5 and the L-Zn-0.05-3 negative electrode prepared in Example 5 and the PDF standard card of pure zinc;

[0025] Figure 4 Graphs showing cycle stability performance of the symmetrical batteries in Application Example 5 and Comparative Application Example 1;

[0026] Figure 5 For Application Examples 1, 5, 6 and Comparative Application Example 1 at 3 mA / cm 2 and 3mAh / cm 2 Cycling stability performance diagram of symmetric cells under test conditions. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] The embodiment of the present invention provides a method for preparing a three-dimensional layered zinc negative electrode, comprising the following steps:

[0030] An inorganic metal salt solution is dropped onto the pure zinc surface, and after standing, washing and drying, a three-dimensional layered zinc negative electrode is obtained.

[0031] The present invention uses an inorganic metal salt solution to treat pure zinc to obtain a zinc negative electrode with a uniform 3D layered structure on the surface, thereby increasing the surface area of ​​the zinc negative electrode and providing more active sites. The introduction of zinc-philic sites helps to reduce the nucleation energy barrier, making Zn 2+The flux is homogenized, thereby increasing the capacity and energy density of the battery; at the same time, it can provide a shorter electron and ion transmission path, reduce the interface resistance; and help to more effectively nest and release zinc ions, increase the storage capacity of the battery, and slow down the rate of battery capacity decay. In addition, the 3D layered structure helps to improve the mechanical stability of the zinc negative electrode and reduce the structural collapse caused by electrode expansion and contraction.

[0032] In a preferred embodiment, the pretreatment method of the pure zinc is: the pure zinc is cleaned three times with deionized water and alcohol in an ultrasonic cleaning machine respectively, and then dried at room temperature.

[0033] In a preferred embodiment, the pure zinc is circular in shape.

[0034] In a preferred embodiment, the inorganic metal salt in the inorganic metal salt solution is ammonium persulfate. The present invention uses ammonium persulfate to etch the zinc negative electrode, and uses the corrosiveness of the ammonium persulfate solution to prepare a 3D layered pure zinc negative electrode; in the process of ammonium persulfate etching the zinc negative electrode, a large amount of active zinc is exposed, which is conducive to the dissolution and deposition of zinc, and homogenizes the electric field and ion flux on the electrode surface, and the 3D layered structure formed by etching increases the effective area and nucleation sites of the zinc negative electrode, and the assembled battery exhibits good electrochemical performance.

[0035] In a preferred embodiment, the concentration of the inorganic metal salt solution is 0.05-3 mol / L, more preferably 0.05-0.3 mol / L. The present invention controls the concentration of the inorganic metal salt solution within the above range, which is conducive to obtaining a three-dimensional layered zinc negative electrode assembled with excellent battery cycle performance. Changing the concentration of the inorganic metal salt solution will reduce the battery cycle performance of the three-dimensional layered zinc negative electrode.

[0036] In a preferred embodiment, the standing temperature is room temperature; the standing time is 1-9 minutes. The present invention controls the standing time within the above range, which is conducive to obtaining a three-dimensional layered zinc negative electrode assembled with excellent electromagnetic cycle performance. Prolonging the standing time will reduce the electroplating or stripping stability of the battery assembled with the three-dimensional layered zinc negative electrode, and shortening the standing time will not achieve the best electroplating or stripping stability of the battery assembled with the three-dimensional layered zinc negative electrode.

[0037] In a preferred embodiment, the washing agent is deionized water; and the washing method is rinsing.

[0038] In a preferred embodiment, the drying method is air-drying at room temperature.

[0039] The present invention provides a three-dimensional layered zinc negative electrode prepared by the preparation method of the three-dimensional layered zinc negative electrode described in the above technical solution.

[0040] In a preferred embodiment, the interlayer distance of the three-dimensional layered zinc negative electrode is 210-290 nm.

[0041] The surface of the three-dimensional layered zinc negative electrode provided by the present invention presents a uniform 3D layered structure.

[0042] The present invention also provides an application of the three-dimensional layered zinc negative electrode described in the above technical solution, and assembles the above three-dimensional layered zinc negative electrode into a symmetrical battery, a hybrid supercapacitor or a full battery.

[0043] In a preferred embodiment, the assembling of the three-dimensional layered zinc negative electrode into a symmetrical battery comprises the following steps: using the three-dimensional layered zinc negative electrode as the positive electrode and the negative electrode, respectively, and assembling them with a separator and an electrolyte into a symmetrical battery.

[0044] In a preferred embodiment, the separator is a glass fiber separator or a cellulose separator.

[0045] In a preferred embodiment, the electrolyte is a ZnSO4 electrolyte, and the concentration of the electrolyte is 1-3 mol / L.

[0046] In a preferred embodiment, the assembling of the three-dimensional layered zinc negative electrode into a hybrid supercapacitor or a full battery comprises the following steps: using the three-dimensional layered zinc as the negative electrode, and assembling it with the positive electrode, electrolyte and separator into a hybrid supercapacitor or a full battery.

[0047] In a preferred embodiment, the positive electrode is AC, CNTs, C, VO2, NaV3O8, V2O5 or MnO2.

[0048] In a preferred embodiment, the electrolyte is a mixed electrolyte composed of a ZnSO4 electrolyte and a MnSO4 electrolyte; the concentration of the ZnSO4 electrolyte is 1-3 mol / L, and the concentration of the MnSO4 electrolyte is 0.01-1 mol / L.

[0049] In a preferred embodiment, the separator is a glass fiber separator or a cellulose separator.

[0050] The room temperature in the embodiments of the present invention refers to "25±2°C".

[0051] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0052] Example 1

[0053] A method for preparing a three-dimensional layered zinc negative electrode is:

[0054] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0055] 2) dissolving 0.228 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.05 mol / L;

[0056] 3) The 0.05 mol / L ammonium persulfate solution obtained in step 2) is added dropwise to the pure zinc electrode obtained in step 1), and the mixture is allowed to stand at room temperature for 1 min. The pure zinc electrode is then rinsed with deionized water and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.05-1 with an interlayer spacing of 210 nm.

[0057] Example 2

[0058] A method for preparing a three-dimensional layered zinc negative electrode is:

[0059] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0060] 2) dissolving 0.456 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.1 mol / L;

[0061] 3) The 0.1 mol / L ammonium persulfate solution obtained in step 2) was added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 1 min, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.1 with an interlayer spacing of 215 nm.

[0062] Example 3

[0063] A method for preparing a three-dimensional layered zinc negative electrode is:

[0064] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0065] 2) dissolving 0.913 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.2 mol / L;

[0066] 3) The 0.2 mol / L ammonium persulfate solution obtained in step 2) is added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 1 min, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.2 with an interlayer spacing of 240-290 nm.

[0067] Example 4

[0068] A method for preparing a three-dimensional layered zinc negative electrode is:

[0069] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0070] 2) dissolving 1.369 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.3 mol / L;

[0071] 3) The 0.3 mol / L ammonium persulfate solution obtained in step 2) was added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 1 min, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.3 with an interlayer spacing of 250 nm.

[0072] Example 5

[0073] A method for preparing a three-dimensional layered zinc negative electrode is:

[0074] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0075] 2) dissolving 0.228 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.05 mol / L;

[0076] 3) The 0.05 mol / L ammonium persulfate solution obtained in step 2) is added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 3 min, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.05-3 with an interlayer spacing of 290 nm.

[0077] Example 6

[0078] A method for preparing a three-dimensional layered zinc negative electrode is:

[0079] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0080] 2) dissolving 0.228 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.05 mol / L;

[0081] 3) The 0.05 mol / L ammonium persulfate solution obtained in step 2) is added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 5 min, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.05-5 with an interlayer spacing of 278 nm.

[0082] Example 7

[0083] A method for preparing a three-dimensional layered zinc negative electrode is:

[0084] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0085] 2) dissolving 0.228 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.05 mol / L;

[0086] 3) The 0.05 mol / L ammonium persulfate solution obtained in step 2) is added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 7 minutes, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.05-7 with an interlayer spacing of 280 nm.

[0087] Example 8

[0088] A method for preparing a three-dimensional layered zinc negative electrode is:

[0089] 1) Pure zinc was cut into discs with a diameter of 12 mm, and then cleaned three times with deionized water and alcohol in an ultrasonic cleaner, and then dried at room temperature to obtain a pure zinc electrode;

[0090] 2) dissolving 0.228 g of ammonium persulfate in 20 mL of deionized water to obtain an ammonium persulfate solution with a concentration of 0.05 mol / L;

[0091] 3) The 0.05 mol / L ammonium persulfate solution obtained in step 2) was added dropwise to the pure zinc electrode obtained in step 1), left at room temperature for 9 minutes, then rinsed with deionized water, and then dried at room temperature to obtain a three-dimensional layered zinc negative electrode L-Zn-0.05-9 with an interlayer spacing of 285 nm.

[0092] Comparative Example 1

[0093] The difference from Example 1 is that ammonium persulfate is replaced by zinc phosphate, and the remaining steps are the same as Example 1, denoted as ZnPO@Zn.

[0094] Comparative Example 2

[0095] The difference from Example 1 is that the concentration of the ammonium persulfate solution is 0.4 mol / L, and the remaining steps are the same as Example 1, recorded as L-Zn-0.4.

[0096] Comparative Example 3

[0097] The difference from Example 1 is that the concentration of the ammonium persulfate solution is 0.5 mol / L, and the remaining steps are the same as Example 1, recorded as L-Zn-0.5.

[0098] Comparative Example 4

[0099] The difference from Example 1 is that, in step 3), the mixture is placed at room temperature for 14 minutes, and the remaining steps are the same as those in Example 1, which are recorded as L-Zn-0.05-14.

[0100] Application Examples 1-8

[0101] The three-dimensional layered zinc negative electrode prepared in Examples 1-8 is respectively the positive electrode and the negative electrode of the battery, and is assembled into a symmetrical battery with a separator and an electrolyte. The separator is glass fiber and the electrolyte is a 2 mol / L ZnSO4 electrolyte.

[0102] Comparative Application Examples 1-5

[0103] The pure zinc negative electrode (i.e., bare zinc electrode) in step 1) of Example 5 or the three-dimensional layered zinc negative electrode prepared in Comparative Examples 1-4 are used as the positive and negative electrodes of the battery, respectively, and are assembled into a symmetrical battery with a diaphragm and an electrolyte. The diaphragm is glass fiber and the electrolyte is a 2 mol / L ZnSO4 electrolyte.

[0104] At 1mA / cm 2 and 1mAh / cm 2 Under the cycle conditions of , the cycle performance of the symmetrical batteries in Application Examples 1-8 and Comparative Application Examples 1-5 were tested, and the results are shown in Table 1.

[0105] Table 1 Cycling performance of symmetrical batteries in application examples 1-8 and comparative application examples 1-5

[0106]

[0107] It can be seen from Table 1 that the symmetrical battery assembled with the three-dimensional layered zinc negative electrode prepared by the preparation method provided in the embodiment of the present invention has excellent cycle performance.

[0108] Figure 1 This is a schematic diagram of the process of preparing a three-dimensional layered zinc negative electrode according to Examples 1-8 of the present invention. The present invention etches the zinc negative electrode by dropping an ammonium persulfate solution onto the surface of pure zinc, and after standing, a zinc negative electrode with a three-dimensional layered structure is obtained.

[0109] Figure 2 The scanning electron microscope images of the pure zinc negative electrode in step 1) of Example 5 and the L-Zn-0.05-3 negative electrode prepared in Example 5 are shown in FIG. a. The pure zinc negative electrode in step 1) of Example 5 and b. The L-Zn-0.05-3 negative electrode prepared in Example 5 are shown in FIG. Figure 2It can be seen that a large amount of active zinc is produced on the surface of the zinc negative electrode after ammonium persulfate treatment, which increases the effective area of ​​the zinc negative electrode, and the surface presents a uniform 3D layered structure with an interlayer spacing of 290nm. This layered structure can shorten the ion transmission path and promote Zn 2+ Fast transmission.

[0110] Figure 3 The X-ray diffraction patterns of the pure zinc negative electrode in step 1) of Example 5 and the L-Zn-0.05-3 negative electrode prepared in Example 5 and the PDF standard card of pure zinc, wherein L-Zn represents the L-Zn-0.05-3 negative electrode prepared in Example 5, pure zinc represents the pure zinc negative electrode in step 1) of Example 5, and PDF#01-0581Zn represents the PDF standard card of pure zinc. Figure 3 It can be seen that the etched zinc negative electrode completely corresponds to the PDF standard card of pure zinc, proving that ammonium persulfate etching only changes the morphology of the zinc negative electrode.

[0111] Figure 4 : is a cycle stability performance diagram of the symmetrical battery in Application Example 5 and Comparative Application Example 1, wherein L-Zn-0.05-3 represents Application Example 5 and pure zinc represents Comparative Application Example 1. Figure 4 It can be seen that at 1mA / cm 2 and 1mAh / cm 2 Under the cycling conditions, the cycling performance of L-Zn-0.05-3 symmetric battery (3000h) is much higher than that of pure zinc symmetric battery (200h), indicating that L-Zn-0.05-3 has good interface stability.

[0112] Figure 5 The figure is a cycle stability performance diagram of the symmetrical battery in Application Examples 1, 5, 6 and Comparative Application Example 1, wherein L-Zn-0.05-1 represents Application Example 1, L-Zn-0.05-3 represents Application Example 5, L-Zn-0.05-5 represents Application Example 6, and pure zinc represents Comparative Application Example 1. Figure 5 It can be seen that at 3mA / cm 2 and 3mAh / cm 2 Under the cycling conditions, the cycling performance of L-Zn-0.05-1 symmetric battery is 90h, the cycling performance of L-Zn-0.05-3 symmetric battery is 600h, the cycling performance of L-Zn-0.05-5 symmetric battery is 10h, and the cycling performance of pure zinc symmetric battery is 60h, indicating that L-Zn-0.05-3 has good interface stability.

[0113] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a three-dimensional layered zinc negative electrode, characterized in that: The following steps are involved: An inorganic metal salt solution is dropped onto the pure zinc surface, and after standing, washing and drying, a three-dimensional layered zinc negative electrode is obtained.

2. The method for preparing a three-dimensional layered zinc negative electrode according to claim 1, characterized in that: The inorganic metal salt in the inorganic metal salt solution is ammonium persulfate.

3. The method for preparing a three-dimensional layered zinc negative electrode according to claim 1, characterized in that: The concentration of the inorganic metal salt solution is 0.05-3 mol / L.

4. The method for preparing a three-dimensional layered zinc negative electrode according to claim 3, characterized in that: The concentration of the inorganic metal salt solution is 0.05-0.3 mol / L.

5. The method for preparing a three-dimensional layered zinc negative electrode according to claim 1, characterized in that: The standing temperature is room temperature, and the standing time is 1-9 minutes.

6. A three-dimensional layered zinc negative electrode prepared by the method for preparing a three-dimensional layered zinc negative electrode according to any one of claims 1 to 5.

7. The use of the three-dimensional layered zinc negative electrode as claimed in claim 6, characterized in that: The three-dimensional layered zinc negative electrode according to claim 6 is assembled into a symmetrical battery, a hybrid supercapacitor or a full battery.

8. The use of the three-dimensional layered zinc negative electrode according to claim 7, characterized in that: The method of assembling a three-dimensional layered zinc negative electrode into a symmetrical battery comprises the following steps: using the three-dimensional layered zinc negative electrode as a positive electrode and a negative electrode, respectively, and assembling them with a separator and an electrolyte into a symmetrical battery.

9. The use of the three-dimensional layered zinc negative electrode according to claim 7, characterized in that: The method of assembling a three-dimensional layered zinc negative electrode into a hybrid supercapacitor or a full battery comprises the following steps: using the three-dimensional layered zinc as the negative electrode, assembling it with a positive electrode, an electrolyte and a separator into a hybrid supercapacitor or a full battery.

10. Use of the three-dimensional layered zinc negative electrode according to claim 8 or 9, characterized in that: The separator is a glass fiber separator or a cellulose separator.

Citation Information

Patent Citations

  • Chromate-free passivator for zinc coating

    CN103205742A

  • Preparation method and application of three-dimensional network structure nanolayer zinc negative electrode

    CN110444730A

  • Negative current collector, battery cell, battery pack, vehicle and processing method of negative current collector

    CN115911400A

  • Preparation and application of tin-protected three-dimensional zinc metal negative electrode with high cycling stability

    CN116315180A