Pole piece, preparation method of pole piece and lithium ion battery

Through the gradient design of the particle size and slurry solid content of the lithium-ion battery pole pieces, the problem of easy cracking of the pole pieces is solved, and the cycle performance and stability of the lithium-ion battery are significantly optimized.

CN118748240APending Publication Date: 2024-10-08JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410745946.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

In the thick coating design of lithium-ion batteries, the pole pieces are prone to cracking, resulting in a decrease in the cycle performance of the lithium-ion battery, and it is difficult to effectively suppress this problem with existing technology.

Method used

Through the gradient design of the particle size on the pole piece, the top layer of the pole piece has large particle size active material, and the gradient design of the solid content of the coating slurry is carried out. The top layer is coated with a high solid content slurry to inhibit cracking of the pole piece.

Benefits of technology

Effectively inhibits pole piece cracking, optimizes the cycle performance of lithium-ion batteries, and improves battery stability and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748240A_ABST
    Figure CN118748240A_ABST
Patent Text Reader

Abstract

The invention provides a pole piece, a preparation method of the pole piece and a lithium ion battery, and the preparation method of the pole piece comprises the following steps: (1) coating two surfaces of a current collector with second slurry containing a second active substance to obtain a pole piece intermediate with a second slurry coating; (2) coating two surfaces of the pole piece intermediate with first slurry containing a first active substance to obtain a wet pole piece with a first slurry coating; (3) drying, rolling and slitting the wet pole piece to obtain a pole piece; wherein the solid content of the first slurry is greater than that of the second slurry, and the particle size D50 of the first active substance is greater than that of the second active substance. The prepared pole piece is not easy to crack in the thick coating processing process, and the cycle performance of the assembled lithium ion battery is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a pole piece, a method for preparing the pole piece, and a lithium ion battery thereof. Background Art

[0002] With the rapid development of lithium-ion batteries, the demand for high-energy-density batteries from the R&D and market sides is getting higher and higher. In specific energy storage fields, based on safety and service life considerations, the optimal direction for high-energy-density systems is to use thick coating technology, and the cost of the battery can be controlled by increasing the coating thickness. However, such designs will face serious processing problems, especially in the coating stage. Thick coating will cause the pole piece to crack easily during processing, and the cracking of the pole piece will lead to a decrease in the cycle performance of the lithium-ion battery.

[0003] Therefore, there is an urgent need to develop an electrode that is not prone to cracking during thick coating, thereby improving the cycle performance of lithium-ion batteries. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a pole piece, a method for preparing the pole piece and a lithium ion battery thereof. The present invention performs a gradient design on the particle size on the pole piece so that the top layer of the pole piece has a large particle size active material, effectively optimizes the surface energy of the material, controls the wetting effect, and thus effectively inhibits the cracking of the pole piece and optimizes the cycle performance of the lithium ion battery; performs a gradient design on the solid content of the coating slurry so that the top layer of the pole piece is coated with a slurry with a high solid content, which is beneficial to the rapid volatilization of the solvent in the slurry, thereby effectively inhibiting the cracking of the pole piece and optimizing the cycle performance of the lithium ion battery.

[0005] Specifically, the present invention provides a method for preparing a pole piece, the method comprising a method for preparing a positive pole piece and / or a method for preparing a negative pole piece;

[0006] The method for preparing the positive electrode sheet comprises the following steps:

[0007] (1) coating a second positive electrode slurry containing a second positive electrode active material on both surfaces of the positive electrode current collector to obtain a positive electrode sheet intermediate having a second positive electrode slurry coating;

[0008] (2) coating a first positive electrode slurry containing a first positive electrode active material on both surfaces of the positive electrode sheet intermediate to obtain a wet positive electrode sheet having a first positive electrode slurry coating;

[0009] (3) drying, rolling, and slitting the wet positive electrode sheet to obtain a positive electrode sheet having a first positive electrode coating layer and a second positive electrode coating layer, wherein the first positive electrode coating layer is converted from the first positive electrode slurry coating layer, and the second positive electrode coating layer is converted from the second positive electrode slurry coating layer;

[0010] Wherein, the solid content of the first positive electrode slurry is greater than the solid content of the second positive electrode slurry; preferably, the solid content of the first positive electrode slurry is 60wt% to 70wt%, and the solid content of the second positive electrode slurry is 50wt% to 60wt%;

[0011] The particle size D50 of the first positive electrode active material is greater than the particle size D50 of the second positive electrode active material; preferably, the particle size D50 of the first positive electrode active material is 1.2 to 2.5 μm, and the particle size D50 of the second positive electrode active material is 0.2 to 1.2 μm;

[0012] The method for preparing the negative electrode sheet comprises the following steps:

[0013] (1′) coating a second negative electrode slurry containing a second negative electrode active material on both surfaces of the negative electrode current collector to obtain a negative electrode sheet intermediate having a second negative electrode slurry coating;

[0014] (2′) coating the first negative electrode slurry containing the first negative electrode active material on both surfaces of the negative electrode sheet intermediate to obtain a wet negative electrode sheet having a first negative electrode slurry coating;

[0015] (3′) drying, rolling, and cutting the wet negative electrode sheet to obtain a negative electrode sheet having a first negative electrode coating layer and a second negative electrode coating layer, wherein the first negative electrode coating layer is formed by converting the first negative electrode slurry coating layer, and the second negative electrode coating layer is formed by converting the second negative electrode slurry coating layer;

[0016] Wherein, the solid content of the first negative electrode slurry is greater than the solid content of the second negative electrode slurry; preferably, the solid content of the first negative electrode slurry is 45wt% to 58wt%, and the solid content of the second negative electrode slurry is 30wt% to 45wt%;

[0017] The particle size D50 of the first negative electrode active material is greater than the particle size D50 of the second negative electrode active material; preferably, the particle size D50 of the first negative electrode active material is 13-25 μm, and the particle size D50 of the second negative electrode active material is 4-13 μm.

[0018] In one or more embodiments, the solid content of the first cathode slurry is 63 wt % to 67 wt %.

[0019] In one or more embodiments, the solid content of the second positive electrode slurry is 56 wt % to 60 wt %.

[0020] In one or more embodiments, the particle size D50 of the first positive active material is 1.2 to 1.8 μm.

[0021] In one or more embodiments, the particle size D50 of the second positive active material is 0.5 to 1.2 μm.

[0022] In one or more embodiments, the solid content of the first negative electrode slurry is 50 wt % to 54 wt %.

[0023] In one or more embodiments, the solid content of the second negative electrode slurry is 38 wt % to 42 wt %.

[0024] In one or more embodiments, the particle size D50 of the first negative electrode active material is 13 to 18 μm.

[0025] In one or more embodiments, the particle size D50 of the second negative electrode active material is 6 to 10 μm.

[0026] In one or more embodiments, the second positive electrode slurry contains 90wt% to 98wt% of the second positive electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the second positive electrode slurry contains 95wt% to 98wt% of the second positive electrode active material, 1wt% to 3wt% of the binder and 1.5wt% to 2.5wt% of the conductive agent.

[0027] In one or more embodiments, the first positive electrode slurry contains 90wt% to 98wt% of the first positive electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the first positive electrode slurry contains 95wt% to 98wt% of the first positive electrode active material, 1wt% to 3wt% of the binder and 1.5wt% to 2.5wt% of the conductive agent.

[0028] In one or more embodiments, the second negative electrode slurry comprises 90wt% to 98wt% of the second negative electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the second negative electrode slurry comprises 95wt% to 97wt% of the second negative electrode active material, 1.5wt% to 3wt% of the binder and 0.5wt% to 2.5wt% of the conductive agent.

[0029] In one or more embodiments, the first negative electrode slurry comprises 90 wt% to 98 wt% of the first negative electrode active material, 0.1 wt% to 3 wt% of a binder, and 0.1 wt% to 3 wt% of a conductive agent. Preferably, the first negative electrode slurry comprises 95 wt% to 97 wt% of the first negative electrode active material, 1.5 wt% to 3 wt% of a binder, and 0.5 wt% to 2.5 wt% of a conductive agent.

[0030] In one or more embodiments, the second positive electrode active material and the second positive electrode active material are each independently selected from one or more of lithium iron phosphate.

[0031] In one or more embodiments, the second negative electrode active material and the second negative electrode active material are each independently selected from one or more of graphite.

[0032] In one or more embodiments, the width of the second positive electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm.

[0033] In one or more embodiments, the thickness of a single surface of the second positive electrode coating layer is 10 to 400 μm, preferably 50 to 200 μm.

[0034] In one or more embodiments, the width of the first positive electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm.

[0035] In one or more embodiments, the single-side thickness of the first positive electrode coating layer is 5 to 100 μm, preferably 10 to 50 μm.

[0036] In one or more embodiments, the width of the second negative electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm.

[0037] In one or more embodiments, the thickness of a single surface of the second negative electrode coating layer is 5 to 200 μm, preferably 10 to 100 μm.

[0038] In one or more embodiments, the width of the first negative electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm.

[0039] In one or more embodiments, the single-side thickness of the first negative electrode coating layer is 5 to 100 μm, preferably 5 to 50 μm.

[0040] The present invention provides a positive electrode sheet or a negative electrode sheet prepared by the preparation method of the present invention.

[0041] The present invention provides a lithium ion battery comprising the positive electrode sheet and / or the negative electrode sheet of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 Schematic diagram of the pole piece structure of some embodiments of the present invention.

[0043] Figure 2 Schematic diagram of the pole piece structure of comparative example 1-2 of the present invention. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0046] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0047] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0048] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0049] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0050] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0051] The present invention provides a positive electrode sheet / negative electrode sheet, the structure of which is as follows Figure 1 shown. Figure 1In the present invention, the pole piece includes a current collector, a second coating layer on both sides of the current collector, and a first coating layer on both sides of the second coating layer. In the present invention, the positive pole piece / negative pole piece shows a gradient distribution trend, and the solid content and active material of the positive pole piece / negative pole piece increase along the current collector, the second coating layer, and the first coating layer. The outermost first coating layer of the positive pole piece / negative pole piece prepared by the present invention has a large-particle active material, which can optimize the surface energy of the material, control the wetting effect, and thus inhibit the cracking of the pole piece and optimize the cycle performance of the lithium-ion battery; and the use of a high-solid content first slurry in the process of the first coating layer during the preparation of the positive pole piece / negative pole piece can promote the rapid volatilization of the solvent, inhibit the cracking of the pole piece, and optimize the cycle performance of the lithium-ion battery.

[0052] The present invention provides a method for preparing a pole piece, and the preparation method includes a method for preparing a positive pole piece and a method for preparing a negative pole piece.

[0053] The method for preparing the positive electrode sheet of the present invention comprises the following steps:

[0054] (1) coating a second positive electrode slurry containing a second positive electrode active material on both surfaces of the positive electrode current collector to obtain a positive electrode sheet intermediate having a second positive electrode slurry coating;

[0055] (2) coating a first positive electrode slurry containing a first positive electrode active material on both surfaces of the positive electrode sheet intermediate to obtain a wet positive electrode sheet having a first positive electrode slurry coating;

[0056] (3) Drying, rolling, and cutting the wet positive electrode sheet to obtain a positive electrode sheet having a first positive electrode coating layer and a second positive electrode coating layer, wherein the first positive electrode coating layer is converted from the first positive electrode slurry coating layer, and the second positive electrode coating layer is converted from the second positive electrode slurry coating layer.

[0057] In the present invention, the solid content of the first positive electrode slurry is greater than the solid content of the second positive electrode slurry. The solvent in the bottom coating area in contact with the current collector of the conventional positive electrode pole piece evaporates quickly, so there is a situation where the bottom is dried earlier and the top layer is too slow to dissipate heat and cannot be dried. Finally, the capillary action produces stress concentration, resulting in cracking of the positive electrode pole piece. The present invention designs the solid content of the positive electrode slurry in a gradient, that is, the second positive electrode slurry with a low solid content is coated in the area in contact with the current collector to obtain the second positive electrode coating layer, and the first positive electrode slurry with a high solid content is coated on the surface of the second positive electrode coating layer in the area not in contact with the current collector to obtain the first positive electrode coating layer. In the preparation process of the positive electrode pole piece, the top layer has a high solid content and the bottom layer has a low solid content. Such a gradient structure is conducive to the rapid volatilization of the solvent, which is conducive to improving the cracking problem of the pole piece and improving the cycle performance of the lithium-ion battery.

[0058] In the present invention, the solid content of the first positive electrode slurry can be 60wt% to 70wt%, preferably 63wt% to 67wt%, such as 63wt%, 64wt%, 65wt%, 66wt%, 67wt%. In the present invention, controlling the solid content of the first positive electrode slurry within the above preferred range is beneficial to suppress the cracking of the positive electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0059] In the present invention, the solid content of the second positive electrode slurry can be 50wt% to 60wt%, preferably 56wt% to 60wt%, such as 56wt%, 57wt%, 58wt%, 59wt%, 60wt%. In the present invention, controlling the solid content of the second positive electrode slurry within the above preferred range is beneficial to suppress the cracking of the positive electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0060] In the present invention, the particle size D50 of the first positive electrode active material is greater than the particle size D50 of the second positive electrode active material. The particle size directly affects the size of its surface energy. The present invention performs a gradient design on the particle size of the positive electrode active material, that is, the second positive electrode slurry containing the second positive electrode active material with a low particle size is coated on the area in contact with the current collector to obtain the second positive electrode coating layer, and the first positive electrode slurry containing the first positive electrode active material with a high particle size is coated on the surface of the second positive electrode coating layer in the area not in contact with the current collector to obtain the first positive electrode coating layer. The positive electrode sheet prepared by this method has a large particle size active material on the top layer and a small particle size active material on the bottom layer. Such a gradient structure can effectively optimize the surface energy of the material, control its wetting effect, inhibit the cracking of the electrode sheet, and improve the cycle performance of the lithium-ion battery.

[0061] In the present invention, the particle size D50 of the first positive electrode active material can be 1.2 to 2.5 μm, preferably 1.2 to 1.8 μm, for example 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm. In the present invention, controlling the particle size D50 of the first positive electrode active material within the above preferred range is beneficial to suppress the cracking of the positive electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0062] In the present invention, the particle size D50 of the second positive electrode active material can be 0.2-1.2 μm, preferably 0.5-1.2 μm, for example 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm. In the present invention, controlling the particle size D50 of the second positive electrode active material within the above preferred range is beneficial to suppress the cracking of the positive electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0063] The method for preparing the negative electrode sheet of the present invention comprises the following steps:

[0064] (1′) coating a second negative electrode slurry containing a second negative electrode active material on both surfaces of the negative electrode current collector to obtain a negative electrode sheet intermediate having a second negative electrode slurry coating;

[0065] (2′) coating a first negative electrode slurry containing a first negative electrode active material on both surfaces of the negative electrode sheet intermediate to obtain a wet negative electrode sheet having a first negative electrode slurry coating;

[0066] (3') Drying, rolling and cutting the wet negative electrode sheet to obtain a positive electrode sheet having a first negative electrode coating layer and a second negative electrode coating layer, wherein the first negative electrode coating layer is converted from the first negative electrode slurry coating layer, and the second negative electrode coating layer is converted from the second negative electrode slurry coating layer.

[0067] In the present invention, the solid content of the first negative electrode slurry is greater than the solid content of the second negative electrode slurry. In the present invention, the solid content of the first negative electrode slurry is greater than the solid content of the second negative electrode slurry. The solvent in the bottom coating area in contact with the current collector of the conventional negative electrode pole piece evaporates quickly, so there is a situation where the bottom is dried earlier and the top layer is too slow to dissipate heat and cannot be dried. Finally, the capillary action produces stress concentration, resulting in cracking of the negative electrode pole piece. The present invention designs the solid content of the negative electrode slurry in a gradient manner, and coats the second negative electrode slurry with a low solid content in the area in contact with the current collector to obtain the second negative electrode coating layer, and coats the first negative electrode slurry with a high solid content on the surface of the second negative electrode coating layer in the area not in contact with the current collector to obtain the first negative electrode coating layer. In the preparation process of the negative electrode pole piece, the top layer has a high solid content and the bottom layer has a low solid content. Such a gradient structure is conducive to the rapid volatilization of the solvent, which is conducive to improving the cracking problem of the pole piece and improving the cycle performance of the lithium-ion battery.

[0068] In the present invention, the solid content of the first negative electrode slurry can be 45wt% to 58wt%, preferably 50wt% to 54wt%, such as 50wt%, 51wt%, 52wt%, 53wt%, 54wt%. In the present invention, controlling the solid content of the first negative electrode slurry within the above preferred range is beneficial to suppress the cracking of the negative electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0069] In the present invention, the solid content of the second negative electrode slurry can be 30wt% to 45wt%, preferably 38wt% to 42wt%, such as 38wt%, 39wt%, 40wt%, 41wt%, 42wt%. In the present invention, controlling the solid content of the second negative electrode slurry within the above preferred range is beneficial to suppress the cracking of the negative electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0070] In the present invention, the particle size D50 of the first negative electrode active material is greater than the particle size D50 of the second negative electrode active material. In the present invention, the particle size D50 of the first negative electrode active material is greater than the particle size D50 of the second negative electrode active material. The particle size directly affects the size of its surface energy. The present invention performs a gradient design on the particle size of the negative electrode active material, that is, the second negative electrode slurry containing the second negative electrode active material with a low particle size is coated in the area in contact with the current collector to obtain the second negative electrode coating layer, and the first negative electrode slurry containing the first negative electrode active material with a high particle size is coated on the surface of the second negative electrode coating layer in the area not in contact with the current collector to obtain the first negative electrode coating layer. The negative electrode pole piece prepared by this method has a large particle size active material on the top layer and a small particle size active material on the bottom layer. Such a gradient structure can effectively optimize the surface energy of the material, control its wetting effect, inhibit the cracking of the pole piece, and improve the cycle performance of the lithium-ion battery.

[0071] In the present invention, the particle size D50 of the first negative electrode active material can be 13 to 25 μm, preferably 13 to 18 μm, for example 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm. In the present invention, controlling the particle size D50 of the first negative electrode active material within the above preferred range is beneficial to suppress the cracking of the negative electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0072] In the present invention, the particle size D50 of the second negative electrode active material can be 4 to 13 μm, preferably 6 to 10 μm, for example 6 μm, 7 μm, 8 μm, 9 μm, 10 μm. In the present invention, controlling the particle size D50 of the second negative electrode active material within the above preferred range is beneficial to suppress the cracking of the negative electrode sheet, thereby improving the cycle performance of the lithium ion battery.

[0073] In the present invention, the second positive electrode slurry contains 90wt% to 98wt% of the second positive electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the second positive electrode slurry contains 95wt% to 98wt% of the second positive electrode active material, 1wt% to 3wt% of the binder and 1.5wt% to 2.5wt% of the conductive agent.

[0074] In the present invention, the first positive electrode slurry contains 90wt% to 98wt% of the first positive electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the first positive electrode slurry contains 95wt% to 98wt% of the first positive electrode active material, 1wt% to 3wt% of the binder and 1.5wt% to 2.5wt% of the conductive agent.

[0075] In some embodiments, the binder in the first positive electrode slurry and the binder in the second positive electrode slurry are of the same type. In some embodiments, the conductive agent in the first positive electrode slurry and the conductive agent in the second positive electrode slurry are of the same type. In some embodiments, the binder in the first positive electrode slurry and the binder in the second positive electrode slurry have the same content. In some embodiments, the conductive agent in the first positive electrode slurry and the conductive agent in the second positive electrode slurry have the same content. In some embodiments, the first positive active material in the first positive electrode slurry and the second positive active material in the second positive electrode slurry are of the same type. In some embodiments, the content of the first positive active material in the first positive electrode slurry and the second positive active material in the second positive electrode slurry is the same.

[0076] In the present invention, the second negative electrode slurry contains 90wt% to 98wt% of the second negative electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the second negative electrode slurry contains 95wt% to 97wt% of the second negative electrode active material, 1.5wt% to 3wt% of the binder and 0.5wt% to 2.5wt% of the conductive agent.

[0077] In the present invention, the first negative electrode slurry contains 90wt% to 98wt% of the first negative electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the first negative electrode slurry contains 95wt% to 97wt% of the first negative electrode active material, 1.5wt% to 3wt% of the binder and 0.5wt% to 2.5wt% of the conductive agent.

[0078] In some embodiments, the binder in the first negative electrode slurry and the binder in the second negative electrode slurry are of the same type. In some embodiments, the conductive agent in the first negative electrode slurry and the conductive agent in the second negative electrode slurry are of the same type. In some embodiments, the binder in the first negative electrode slurry and the binder in the second negative electrode slurry have the same content. In some embodiments, the conductive agent in the first negative electrode slurry and the conductive agent in the second negative electrode slurry have the same content. In some embodiments, the first negative electrode active material in the first negative electrode slurry and the second negative electrode active material in the second negative electrode slurry are of the same type. In some embodiments, the content of the first negative electrode active material in the first negative electrode slurry and the second negative electrode active material in the second negative electrode slurry is the same.

[0079] In the present invention, the second positive electrode active material and the second positive electrode active material can each be independently selected from one or more of lithium iron phosphate.

[0080] In the present invention, the second negative electrode active material and the second negative electrode active material can each be independently selected from one or more of graphite.

[0081] In the present invention, the conductive agent in the first positive electrode slurry and the second positive electrode slurry is one or more of conductive carbon black, carbon nanotubes and graphene.

[0082] In the present invention, the binder in the first positive electrode slurry and the second positive electrode slurry is polyvinylidene fluoride (PVDF).

[0083] In the present invention, the conductive agent in the first negative electrode slurry and the second negative electrode slurry is one or more of conductive carbon black, carbon nanotubes and graphene.

[0084] In the present invention, the binder in the first negative electrode slurry and the second negative electrode slurry is one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber and polyacrylic acid.

[0085] In the present invention, the width of the second positive electrode coating layer may be 20 to 1200 mm, preferably 200 to 400 mm, for example, 200 mm, 250 mm, 300 mm, 350 mm, or 400 mm.

[0086] In the present invention, the thickness of a single surface of the second positive electrode coating layer may be 10 to 400 μm, preferably 50 to 200 μm, for example, 50 μm, 100 μm, 150 μm, or 200 μm.

[0087] In the present invention, the width of the first positive electrode coating layer may be 20 to 1200 mm, preferably 200 to 400 mm, for example, 200 mm, 250 mm, 300 mm, 350 mm, or 400 mm.

[0088] In the present invention, the single-side thickness of the first positive electrode coating layer may be 5 to 100 μm, preferably 10 to 50 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, or 50 μm.

[0089] In the present invention, the width of the second negative electrode coating layer may be 20 to 1200 mm, preferably 200 to 400 mm, for example, 200 mm, 250 mm, 300 mm, 350 mm, or 400 mm.

[0090] In the present invention, the single-sided thickness of the second negative electrode coating layer may be 5 to 200 μm, preferably 10 to 100 μm, for example 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or 100 μm.

[0091] In the present invention, the width of the first negative electrode coating layer may be 20 to 1200 mm, preferably 200 to 400 mm, for example, 200 mm, 250 mm, 300 mm, 350 mm, or 400 mm.

[0092] In the present invention, the single-sided thickness of the first negative electrode coating layer can be 5 to 100 μm, preferably 5 to 50 μm, for example 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm. The present invention provides a lithium-ion battery of a positive electrode sheet and / or a negative electrode sheet of the present invention. In some embodiments, the lithium-ion battery comprises the positive electrode sheet of the present invention, which is beneficial to the improvement of the cycle performance of the lithium-ion battery due to the improvement of the cracking phenomenon of the positive electrode sheet. In some embodiments, the lithium-ion battery comprises the negative electrode sheet of the present invention, which is beneficial to the improvement of the cycle performance of the lithium-ion battery due to the improvement of the cracking phenomenon of the negative electrode sheet. In some embodiments, the lithium-ion battery comprises the positive electrode sheet and the negative electrode sheet of the present invention, and the cracking phenomenon of the positive electrode sheet and the negative electrode sheet is improved, and the cycle performance of the lithium-ion battery is greatly improved.

[0093] In the present invention, the battery cell of the lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0094] The separator in the lithium ion battery of the present invention can be a polymer separator, a ceramic separator or a polymer / ceramic composite separator. The polymer separator includes a single-layer polymer separator and a multi-layer polymer separator. The single-layer polymer separator includes a polyethylene (PE) separator and a polypropylene (PP) separator.

[0095] The electrolyte in the lithium ion battery of the present invention generally comprises a solvent and a lithium salt. The electrolyte suitable for the present invention may be conventional, for example, the solvent may be selected from one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); the lithium salt may be selected from lithium iron phosphate, lithium hexafluorophosphate (LiPF 6 ), lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium tetrafluoroborate (LiBF 4 )

[0096] The present invention laminates and / or winds the positive electrode sheet, the negative electrode sheet and the separator, and packages them in a shell, and then undergoes drying, liquid injection (injection of electrolyte), packaging, standing, formation, and volume separation to obtain a lithium ion battery. The packaging process of the lithium ion battery of the present invention can be cylindrical, square or soft package. The cylindrical packaging generally adopts steel shell packaging, the square packaging generally adopts aluminum alloy and stainless steel packaging, and the soft package packaging generally adopts aluminum plastic film packaging. Therefore, the form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft package lithium ion battery or an aluminum shell lithium ion battery.

[0097] Compared with the prior art, the present invention has the following beneficial effects:

[0098] (1) The present invention designs the particle size on the pole piece in a gradient manner, so that the surface layer of the pole piece has active materials with large particle size, which effectively optimizes the surface energy of the material, controls the wetting effect, and thus effectively inhibits the cracking of the pole piece, thereby further optimizing the cycle performance of the lithium-ion battery;

[0099] (2) The present invention implements a gradient design of the solid content of the coating slurry so that the top layer of the electrode is coated with a slurry with a high solid content, which is beneficial to the rapid volatilization of the solvent in the slurry, thereby effectively inhibiting the cracking of the electrode and further optimizing the cycle performance of the lithium-ion battery.

[0100] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.

[0101] Comparative Example 1

[0102] This comparative example prepares a lithium ion battery according to the following steps:

[0103] (1) Preparation of positive electrode slurry: lithium iron phosphate, PVDF and conductive carbon black are dry-mixed in a mass ratio of 97:2:1, and then N-methylpyrrolidone (NMP) is added and stirred to prepare a positive electrode slurry; wherein the solid content of the positive electrode slurry is 60wt%, and the particle size D50 of the lithium iron phosphate is 1μm;

[0104] (2) Preparation of positive electrode sheet: The positive electrode slurry prepared in step (1) is uniformly coated on both surfaces of the aluminum foil, and the positive electrode sheet consisting of the aluminum foil and the positive electrode material layers on both sides thereof is prepared by drying, rolling and slitting, wherein the single-side thickness of the positive electrode material layer is 120 μm and the width of the positive electrode material layer is 200 mm; the structure of the positive electrode sheet prepared in this comparative example is as follows: Figure 2 As shown;

[0105] (3) Preparation of negative electrode slurry: Graphite, conductive carbon black and sodium carboxymethyl cellulose were dry mixed in a mass ratio of 96:1:1, and then deionized water was added for stirring, and finally styrene-butadiene rubber was added and dispersed evenly (the mass ratio of styrene-butadiene rubber to sodium carboxymethyl cellulose was 2:1) to prepare a negative electrode slurry; wherein the solid content of the negative electrode slurry was 50 wt %, and the particle size D50 of the graphite was 10 μm;

[0106] (4) Preparation of negative electrode sheet: The negative electrode slurry prepared in step (3) is uniformly coated on a copper foil, and dried, rolled, and cut to obtain a negative electrode sheet consisting of a copper foil and negative electrode material layers on both sides thereof, wherein the single-sided thickness of the negative electrode material layer is 80 μm, and the width of the negative electrode material layer is 210 mm; the structure of the negative electrode sheet prepared in this comparative example is as follows: Figure 2 As shown;

[0107] (5) Preparation of lithium-ion battery: The positive electrode sheet prepared in step (2), the negative electrode sheet prepared in step (4) and the polypropylene (PP) substrate separator are wound to obtain a bare battery cell, which is then assembled, dried, and injected with 1.0 mol / L of LiPF 6 The lithium-ion battery is prepared by the following steps: a solvent is an electrolyte containing EC and EMC in a mass ratio of 1:2, and a formation and a capacity separation process.

[0108] Example 1

[0109] This embodiment prepares a lithium ion battery according to the following steps:

[0110] (1) Preparation of the second positive electrode slurry: lithium iron phosphate, PVDF and conductive carbon black were dry-mixed in a mass ratio of 97:2:1, and then NMP was added and stirred to prepare a second positive electrode slurry, wherein the solid content of the second positive electrode slurry was 58 wt %, and the particle size D50 of the lithium iron phosphate was 1 μm;

[0111] (2) Preparation of a positive electrode sheet intermediate: uniformly coating the second positive electrode slurry prepared in step (1) on both surfaces of the aluminum foil to obtain a positive electrode sheet intermediate having a coating of the second positive electrode slurry;

[0112] (3) Preparation of a first positive electrode slurry: dry-mixing lithium iron phosphate, PVDF and conductive carbon black in a mass ratio of 97:2:1, and then adding NMP and stirring to prepare a first positive electrode slurry; wherein the solid content of the first positive electrode slurry is 65wt%, and the particle size D50 of the lithium iron phosphate is 1μm;

[0113] (4) Preparation of a wet positive electrode sheet: coating the first positive electrode slurry prepared in step (3) on both surfaces of the positive electrode sheet intermediate prepared in step (2) to obtain a wet positive electrode sheet having a coating of the first positive electrode slurry;

[0114] (5) Preparation of positive electrode sheet: The wet positive electrode sheet prepared in step (4) is dried, rolled and cut. During the drying and rolling process, the first positive electrode slurry coating is converted into the first positive electrode coating layer, and the second positive electrode slurry coating is converted into the second positive electrode coating layer, so as to obtain a positive electrode sheet consisting of an aluminum foil and the first positive electrode coating layer and the second positive electrode coating layer on both sides thereof, wherein the single-sided thickness of the first positive electrode coating layer is 20 μm, the single-sided thickness of the second positive electrode coating layer is 100 μm, the single-sided total thickness of the first positive electrode coating layer and the second positive electrode coating layer is 120 μm, and the width of the first positive electrode coating layer and the second positive electrode coating layer is 200 mm. The structure of the positive electrode sheet prepared in this embodiment is as follows: Figure 1 shown.

[0115] (6) Preparation of lithium-ion battery: The positive electrode sheet prepared in this example, the negative electrode sheet prepared in comparative example 1 and the PP substrate separator were wound to obtain a bare battery cell, which was then assembled, dried, and injected with 1.0 mol / L of LiPF 6 The lithium-ion battery is prepared by the following steps: a solvent is an electrolyte containing EC and EMC in a mass ratio of 1:2, and a formation and a capacity separation process.

[0116] Example 2

[0117] This embodiment prepares a lithium ion battery according to the following steps:

[0118] (1) Preparation of the second negative electrode slurry: Graphite, conductive carbon black and sodium carboxymethyl cellulose were dry-mixed in a mass ratio of 96:1:1, and then deionized water was added for stirring, and finally 2% by mass of styrene-butadiene rubber was added and dispersed evenly to prepare the second negative electrode slurry, wherein the solid content of the second negative electrode slurry was 48 wt %, and the particle size D50 of the graphite was 10 μm;

[0119] (2) Preparation of a negative electrode sheet intermediate: uniformly coating the second negative electrode slurry prepared in step (1) on both surfaces of the copper foil to obtain a negative electrode sheet intermediate having a second negative electrode slurry coating;

[0120] (3) Preparation of the first negative electrode slurry: Graphite, conductive carbon black and sodium carboxymethyl cellulose are dry-mixed in a mass ratio of 96:1:1, and then deionized water is added for stirring, and finally styrene-butadiene rubber is added and dispersed evenly (the mass ratio of styrene-butadiene rubber to sodium carboxymethyl cellulose is 2:1) to prepare a first negative electrode slurry; wherein the solid content of the first negative electrode slurry is 55 wt %, and the particle size D50 of the graphite is 10 μm;

[0121] (4) Preparation of a wet negative electrode sheet: coating the first negative electrode slurry prepared in step (3) on both surfaces of the negative electrode sheet intermediate prepared in step (2) to obtain a wet negative electrode sheet having a first negative electrode slurry coating;

[0122] (5) Preparation of negative electrode sheet: The wet negative electrode sheet prepared in step (4) is dried, rolled and cut. During the drying and rolling process, the first negative electrode slurry coating is converted into the first negative electrode coating layer, and the second negative electrode slurry coating is converted into the second negative electrode coating layer, so as to obtain a negative electrode sheet consisting of a copper foil and the first negative electrode coating layer and the second negative electrode coating layer on both sides thereof, wherein the single-side thickness of the first negative electrode coating layer is 10 μm, the single-side thickness of the second negative electrode coating layer is 70 μm, the single-side total thickness of the first negative electrode coating layer and the second negative electrode coating layer is 80 μm, and the width of the first negative electrode coating layer and the second negative electrode coating layer is 210 mm. The structure of the negative electrode sheet prepared in this embodiment is as follows: Figure 1 shown.

[0123] (6) Preparation of lithium-ion battery: The positive electrode sheet prepared in Comparative Example 1, the negative electrode sheet prepared in this embodiment and the PP substrate separator were wound to obtain a bare battery cell, which was then assembled, dried, and injected with 1.0 mol / L of LiPF 6 The lithium-ion battery is prepared by the following steps: a solvent is an electrolyte containing EC and EMC in a mass ratio of 1:2, and a formation and a capacity separation process.

[0124] Example 3

[0125] The other conditions of this embodiment are the same as those of Embodiment 1, and the only difference is that the negative electrode plate is replaced by the negative electrode plate prepared in Embodiment 2.

[0126] Comparative Example 2

[0127] The other conditions of this comparative example are the same as those of comparative example 1, except that the particle size D50 of lithium iron phosphate is replaced from 1.0 μm to 1.5 μm, and the particle size D50 of graphite is replaced from 10 μm to 15 μm.

[0128] Example 4

[0129] The other conditions of this embodiment are the same as those of Embodiment 1, except that the particle size D50 of the lithium iron phosphate in the first positive electrode slurry is replaced from 1.0 μm to 1.5 μm.

[0130] Example 5

[0131] The other conditions of this embodiment are the same as those of Embodiment 2, except that the particle size D50 of the graphite in the first negative electrode slurry is replaced from 10 μm to 15 μm.

[0132] Example 6

[0133] The other conditions of this embodiment are the same as those of Embodiment 4, the only difference being that the negative electrode plate is replaced with the negative electrode plate prepared in Embodiment 5.

[0134] Comparative Example 3

[0135] The other conditions of this comparative example are the same as those of Example 1, except that the particle size D50 of the lithium iron phosphate in the second positive electrode slurry is replaced from 1.0 μm to 1.5 μm.

[0136] Comparative Example 4

[0137] The other conditions of this embodiment are the same as those of Embodiment 2, except that the particle size D50 of the graphite in the second negative electrode slurry is replaced from 10 μm to 15 μm.

[0138] Test Case

[0139] Cracking test: The pole pieces prepared in Examples 1-6 and Comparative Examples 1-4 were cut into 15 m pieces and placed on the platform area, and the number of cracks in the pole pieces was visually counted with the help of a flashlight (the coating speed for pole piece preparation was kept at 11 m / min). The cracking test results of the pole pieces prepared in Examples 1-6 and Comparative Examples 1-4 are shown in Table 1-2.

[0140] Cyclic capacity retention rate test: According to GB / T 36276-2018, the lithium ion batteries prepared in Examples 1-6 and Comparative Examples 1-4 were tested for cyclic capacity retention rate, the first step: at 45°C, constant current charging to 3.65V, constant voltage, cut-off current 0.05C; the second step: standing for 10min; the third step: 0.5C constant current discharge to 2.5V; the fourth step: standing for 10min; the fifth step: cycle the first step to the fourth step until the battery capacity retention rate is less than 80%. The test results of the cyclic capacity retention rate of the lithium ion batteries prepared in Examples 1-6 and Comparative Examples 1-4 are shown in Table 1-2.

[0141] Table 1 Cracking of the pole pieces prepared in Examples 1-6 and cycle capacity retention of the assembled lithium-ion batteries

[0142]

[0143] Table 2 Cracking of pole pieces prepared in Comparative Examples 1-4 and cycle capacity retention of assembled lithium-ion batteries

[0144]

[0145]

[0146] As can be seen from Tables 1 and 2, compared with Comparative Example 1 in which the solid content of the positive electrode slurry is not designed, the positive electrode plate has a low degree of cracking and the assembled lithium ion battery has excellent cycle performance by gradient design of the solid content of the positive electrode slurry so that the top layer of the positive electrode plate is coated with a high solid content slurry. Compared with Example 1 in which the positive electrode slurry solid content is gradient designed so that the top layer of the positive electrode plate is coated with a high solid content slurry, the positive electrode plate has a lower degree of cracking and the assembled lithium ion battery has better cycle performance by gradient design of the particle size on the positive electrode plate. This further proves that the positive electrode plate prepared by the present invention has a large particle size active material on the top layer of the plate, and the positive electrode plate with a high solid content slurry on the top layer of the plate is not easy to crack, and the assembled lithium ion battery has excellent cycle performance.

Claims

1. A method for preparing a pole piece, characterized in that: The preparation method includes a preparation method of a positive electrode sheet and / or a preparation method of a negative electrode sheet; The method for preparing the positive electrode sheet comprises the following steps: (1) coating a second positive electrode slurry containing a second positive electrode active material on both surfaces of the positive electrode current collector to obtain a positive electrode sheet intermediate having a second positive electrode slurry coating; (2) coating a first positive electrode slurry containing a first positive electrode active material on both surfaces of the positive electrode sheet intermediate to obtain a wet positive electrode sheet having a first positive electrode slurry coating; (3) drying, rolling, and slitting the wet positive electrode sheet to obtain a positive electrode sheet having a first positive electrode coating layer and a second positive electrode coating layer, wherein the first positive electrode coating layer is converted from the first positive electrode slurry coating layer, and the second positive electrode coating layer is converted from the second positive electrode slurry coating layer; Wherein, the solid content of the first positive electrode slurry is greater than the solid content of the second positive electrode slurry; preferably, the solid content of the first positive electrode slurry is 60wt% to 70wt%, and the solid content of the second positive electrode slurry is 50wt% to 60wt%; The particle size D50 of the first positive electrode active material is greater than the particle size D50 of the second positive electrode active material; preferably, the particle size D50 of the first positive electrode active material is 1.2 to 2.5 μm, and the particle size D50 of the second positive electrode active material is 0.2 to 1.2 μm; The method for preparing the negative electrode sheet comprises the following steps: (1′) coating a second negative electrode slurry containing a second negative electrode active material on both surfaces of the negative electrode current collector to obtain a negative electrode sheet intermediate having a second negative electrode slurry coating; (2′) coating the first negative electrode slurry containing the first negative electrode active material on both surfaces of the negative electrode sheet intermediate to obtain a wet negative electrode sheet having a first negative electrode slurry coating; (3′) drying, rolling, and cutting the wet negative electrode sheet to obtain a negative electrode sheet having a first negative electrode coating layer and a second negative electrode coating layer, wherein the first negative electrode coating layer is formed by converting the first negative electrode slurry coating layer, and the second negative electrode coating layer is formed by converting the second negative electrode slurry coating layer; Wherein, the solid content of the first negative electrode slurry is greater than the solid content of the second negative electrode slurry; preferably, the solid content of the first negative electrode slurry is 45wt% to 58wt%, and the solid content of the second negative electrode slurry is 30wt% to 45wt%; The particle size D50 of the first negative electrode active material is greater than the particle size D50 of the second negative electrode active material; preferably, the particle size D50 of the first negative electrode active material is 13-25 μm, and the particle size D50 of the second negative electrode active material is 4-13 μm.

2. The preparation method according to claim 1, characterized in that The preparation method has one or more of the following characteristics: The solid content of the first positive electrode slurry is 63wt% to 67wt%; The solid content of the second positive electrode slurry is 56wt% to 60wt%; The particle size D50 of the first positive electrode active material is 1.2 to 1.8 μm; The particle size D50 of the second positive electrode active material is 0.5 to 1.2 μm; The solid content of the first negative electrode slurry is 50wt% to 54wt%; The solid content of the second negative electrode slurry is 38wt% to 42wt%; The particle size D50 of the first negative electrode active material is 13 to 18 μm; The particle size D50 of the second negative electrode active material is 6 to 10 μm.

3. The preparation method according to claim 1, characterized in that: The second positive electrode slurry comprises 90 wt% to 98 wt% of the second positive electrode active material, 0.1 wt% to 3 wt% of the binder and 0.1 wt% to 3 wt% of the conductive agent, preferably, the second positive electrode slurry comprises 95 wt% to 98 wt% of the second positive electrode active material, 1 wt% to 3 wt% of the binder and 1.5 wt% to 2.5 wt% of the conductive agent; and / or The first positive electrode slurry contains 90wt% to 98wt% of the first positive electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the first positive electrode slurry contains 95wt% to 98wt% of the first positive electrode active material, 1wt% to 3wt% of the binder and 1.5wt% to 2.5wt% of the conductive agent.

4. The preparation method according to claim 1, characterized in that: The second negative electrode slurry comprises 90 wt% to 98 wt% of the second negative electrode active material, 0.1 wt% to 3 wt% of a binder and 0.1 wt% to 3 wt% of a conductive agent. Preferably, the second negative electrode 243820 The slurry comprises 95 wt% to 97 wt% of the second negative electrode active material, 1.5 wt% to 3 wt% of a binder and 0.5 wt% to 2.5 wt% of a conductive agent; and / or The first negative electrode slurry contains 90wt% to 98wt% of the first negative electrode active material, 0.1wt% to 3wt% of the binder and 0.1wt% to 3wt% of the conductive agent. Preferably, the first negative electrode slurry contains 95wt% to 97wt% of the first negative electrode active material, 1.5wt% to 3wt% of the binder and 0.5wt% to 2.5wt% of the conductive agent.

5. The preparation method according to claim 1, characterized in that: The second positive electrode active material and the second positive electrode active material are each independently selected from one or more of lithium iron phosphate.

6. The preparation method according to claim 1, characterized in that: The second negative electrode active material and the second negative electrode active material are each independently selected from one or more of graphite.

7. The preparation method according to claim 1, characterized in that: The preparation method has one or more of the following characteristics: The width of the second positive electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm; The single-side thickness of the second positive electrode coating layer is 10 to 400 μm, preferably 50 to 200 μm; The width of the first positive electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm; The single-side thickness of the first positive electrode coating layer is 5 to 100 μm, preferably 10 to 50 μm.

8. The preparation method according to claim 1, characterized in that: The preparation method has one or more of the following characteristics: The width of the second negative electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm; The single-side thickness of the second negative electrode coating layer is 5 to 200 μm, preferably 10 to 100 μm; The width of the first negative electrode coating layer is 20 to 1200 mm, preferably 200 to 400 mm; The single-side thickness of the first negative electrode coating layer is 5 to 100 μm, preferably 5 to 50 μm.

9. A positive electrode sheet or a negative electrode sheet prepared by the preparation method according to any one of claims 1 to 8.

10. A lithium ion battery comprising the positive electrode sheet and / or the negative electrode sheet according to claim 9.