Electrode material with excellent expansion resistance and preparation method and application thereof
Preparation by high-temperature mixed hydrothermal method of H2V3O8/MXene/VO2 heterojunction materials solves the problems of poor ion diffusivity and sluggish kinetics of vanadium oxide materials in zinc-ion batteries, and achieves excellent expansion resistance and high specific capacity , providing efficient cathode materials for zinc-ion batteries.
Patent Information
- Application Number
- CN202410844639.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The poor ion diffusivity, slow kinetics and structural damage caused by Zn2+ intercalation/extraction of vanadium oxide materials in zinc-ion batteries limit their application in aqueous zinc-ion batteries.
The H2V3O8/MXene/VO2 heterojunction material is prepared by a high-temperature mixed hydrothermal method. The built-in electric field of the heterojunction is used to accelerate ion diffusion and the nanorod-shaped H2V3O8/MXene and VO2 are evenly distributed on the surface of the MXene nanosheets to form a heterogeneous material. The volume changes of the junction material are opposite during the charge and discharge process, which alleviates the volume expansion and improves the expansion resistance.
It significantly improves the conductivity and specific capacity of the electrode material, simplifies the preparation process, reduces the cost, alleviates the volume expansion problem during charge and discharge, and provides an excellent cathode material for zinc-ion batteries.
Smart Images

Figure CN118748245A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrode material, a preparation method and an application thereof, and in particular to an electrode material with excellent expansion resistance, a preparation method and an application thereof. Background Art
[0002] In recent years, the large-scale consumption of traditional fossil fuels has increasingly aggravated environmental pollution. Therefore, the demand for clean energy is increasing, and there is an urgent need to develop safe and environmentally friendly electrochemical energy storage systems. Aqueous zinc-ion batteries (ZIBs) have low redox potential and high theoretical specific capacity (820 mAh g -1 ), low cost (low price of Zn) and easy assembly have attracted much attention. In addition, the aqueous electrolyte used in zinc-ion batteries is non-toxic and very environmentally friendly. However, the slow kinetics of zinc ions has always hindered its further development. Therefore, the development of positive electrode materials with high specific capacity and long cycle life is a top priority for zinc-ion batteries. To date, manganese-based oxides, Prussian blue, transition metal sulfides and vanadium oxides have been widely used in zinc-ion battery positive electrode materials. Among them, vanadium oxide materials have good adaptability in battery systems due to their advantages such as multiple redox states, open crystal structure and high theoretical specific capacity. However, their poor ion diffusivity, slow kinetics and Zn 2+ The strain-induced structural damage of vanadium oxide caused by repeated insertion / extraction in the lattice has greatly limited its further application in ZIBs. Therefore, it is crucial to modify vanadium oxide materials to improve their structural stability and cycling performance to meet the practical application conditions of ZIBs. Summary of the Invention
[0003] Purpose of the invention: The first purpose of the present invention is to provide an electrode material with excellent expansion resistance; the second purpose of the present invention is to provide a one-step high-temperature mixed hydrothermal method for preparing the above-mentioned electrode material; the third purpose of the present invention is to provide the use of the above-mentioned electrode material as a positive electrode material in a zinc ion battery.
[0004] Technical Solution: The electrode material with excellent expansion resistance described in this invention is a H2V3O8 / MXene / VO2 heterojunction material. During charge and discharge, the lattice changes of H2V3O8 / MXene and VO2 / MXene are opposite (during discharge, the volume of H2V3O8 / MXene shrinks, while the volume of VO2 / MXene expands; during charge, the volume of H2V3O8 / MXene expands, while the volume of VO2 / MXene shrinks). This fully mitigates the volume expansion of the heterojunction material during charge and discharge, resulting in excellent expansion resistance. The formation of a built-in electric field in the heterojunction accelerates ion diffusion dynamics and induces more active sites.
[0005] Furthermore, nanorod-shaped H2V3O8 / MXene and VO2 / MXene are evenly distributed on the surface of MXene nanosheets, forming H2V3O8 / MXene / VO2 heterojunction materials.
[0006] The method for preparing the electrode material with excellent expansion resistance according to the present invention comprises the following steps:
[0007] (1) Prepare H2V3O8 / MXene aqueous solution as liquid A and VO2 / MXene aqueous solution as liquid B;
[0008] (2) placing liquid A and liquid B in a hydrothermal reactor with different reaction chambers and heating them;
[0009] (3) When the temperature reaches the reaction temperature, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is in a rotating state during the reaction process, and the target material is prepared after the reaction.
[0010] Furthermore, in step (1), the concentration of the H2V3O8 / MXene aqueous solution is 0.01 to 0.05 g / mL.
[0011] Furthermore, in step (2), the concentration of the VO2 / MXene aqueous solution is 0.01 to 0.05 g / mL.
[0012] Furthermore, in step (3), the rotation speed is controlled at 10-15 rpm, and the hydrothermal reaction temperature is 180-240°C.
[0013] Furthermore, after the reaction is completed, the reactor is continuously stirred and cooled to room temperature, and then filtered, washed, and dried to obtain a black powder electrode material.
[0014] The present invention further protects the application of the electrode material as a positive electrode material in a zinc ion battery.
[0015] The preparation principle of the present invention is as follows: using H2V3O8 / MXene and VO2 / MXene as raw materials and water as solvent, a H2V3O8 / MXene / VO2 composite material with a heterogeneous structure is synthesized through a one-step high-temperature mixing hydrothermal method. The high-temperature mixing hydrothermal method can effectively improve the crystallinity and purity of the product and avoid the generation of other impurities during the heating process. Through high-temperature rotary mixing technology, H2V3O8 / MXene and VO2 / MXene can be effectively compounded to form a heterogeneous structure. The successful construction of the heterojunction material enables the charge to be redistributed at the interface, and the formation of a built-in electric field accelerates the ion diffusion dynamics and induces more active sites. At the same time, the volume changes of the two raw materials, H2V3O8 / MXene and VO2 / MXene, during the charge and discharge process are opposite. Combining the two can fully alleviate the overall volume expansion of the positive electrode, making it have excellent expansion resistance.
[0016] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The electrode material has excellent expansion resistance. The present invention constructs a heterostructure of two materials with opposite volume changes during charging and discharging, which fully alleviates the volume expansion during charging and discharging, making it have excellent expansion resistance; at the same time, the formation of the built-in electric field in the heterojunction accelerates the ion diffusion dynamics and induces more active sites, effectively improving the conductivity and specific capacity of the electrode material; (2) The H2V3O8 / MXene / VO2 zinc ion battery positive electrode material is synthesized by a one-step high-temperature mixed hydrothermal method, which not only simplifies the experimental process and reduces the experimental cost, but also improves the conductivity and structural stability of the material, alleviates the problem of volume expansion during charging and discharging, and provides an excellent positive electrode material for the application of aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Flow chart for the preparation of H2V3O8 / MXene / VO2 electrode materials with heterostructure;
[0018] Figure 2 This is the SEM image of the H2V3O8 / MXene / VO2 electrode material prepared in Example 1;
[0019] Figure 3 TEM image of the H2V3O8 / MXene / VO2 electrode material prepared in Example 1;
[0020] Figure 4 The H2V3O8 / MXene / VO2 electrode in Example 1 and the positive electrode materials in Examples 2 and 3 are 0.1Ag -1 Cycling performance diagram at current density of ;
[0021] Figure 5The H2V3O8 / MXene / VO2 electrode in Example 1 and the positive electrode materials in Examples 4 and 5 are 0.1Ag -1 Cycling performance diagram at current density of ;
[0022] Figure 6 The H2V3O8 / MXene / VO2 electrode in Example 1 and the positive electrode materials of Comparative Examples 1 and 2 are 0.1Ag -1 Cycling performance diagram at current density of ;
[0023] Figure 7 XRD patterns of the H2V3O8 / MXene / VO2 electrode prepared in Example 1 at different charge and discharge stages;
[0024] Figure 8 Schematic diagram of compounding two materials with opposite volume changes during the charge and discharge process. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0026] Example 1
[0027] A method for preparing a positive electrode material for a zinc ion battery with excellent expansion resistance, the preparation process is as follows Figure 1 The specific steps are as follows:
[0028] Step 1) Add 0.1 g H2V3O8 / MXene to 10 mL aqueous solution and ultrasonicate for 10 min to prepare solution A (the preparation method of H2V3O8 / MXene is the same as that of Comparative Example 1, refer to the literature: Penghua Liang, Tengfei Xu, Kongjun Zhu, *etal. Heterogeneous interface-boosted zinc storage of H2V3O8 nanowire / Ti3C2T x MXene composite towards high-rate and long cycle lifespan aqueous zinc-ionbatteries, Energy Storage Materials, 2022, 50, 63-74.);
[0029] Step 2) Add 0.1 g VO2 / MXene to 10 mL aqueous solution and ultrasonicate for 10 min to prepare solution B (the preparation method of VO2 / MXene is the same as that of Comparative Example 2, refer to the literature: Penghua Liang, Kongjun Zhu*, Jiatao Chen et al. Oxygen vacancies and heterointerface co-boosted Zn 2+ (De)intercalationkinetics in VO2 for ultra-efficient aqueous zinc-ion batteries, Journal of Power Sources, 2023, 568, 232945.);
[0030] Step 3) Place Liquid A and Liquid B in separate hydrothermal reactor chambers (total volume 60 ml). Seal the hydrothermal reactor and heat in an oven. Ensure that Liquid A and Liquid B do not come into contact during heating until the reaction temperature is reached.
[0031] Step 4) When the reaction temperature in step 3) rises to 200°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 200°C for 1 hour.
[0032] Step 5) The reactor was continuously stirred and cooled to room temperature, and black powder of the H2V3O8 / MXene / VO2 heterojunction material was obtained after filtration, washing, and drying.
[0033] See also Figure 2 It can be seen that the morphology of the prepared H2V3O8 / MXene / VO2 electrode is a composite structure of H2V3O8, VO2 nanorods and MXene nanosheets. Figure 3 , the composite of MXene nanosheets and nanorods of different thicknesses can be seen more clearly.
[0034] Example 2
[0035] Step 1) Add 0.2 g H2V3O8 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to obtain solution A;
[0036] Step 2) Add 0.1 g of VO2 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to prepare solution B;
[0037] Step 3) Place Liquid A and Liquid B in separate hydrothermal reactor chambers (total volume 60 ml). Seal the hydrothermal reactor and heat in an oven. Ensure that Liquid A and Liquid B do not come into contact during heating until the reaction temperature is reached.
[0038] Step 4) When the reaction temperature in step 3) rises to 200°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 200°C for 1 hour.
[0039] Step 5) The reactor was continuously stirred and cooled to room temperature, and black powder of the H2V3O8 / MXene / VO2 heterojunction material was obtained after filtration, washing, and drying.
[0040] Example 3
[0041] Step 1) Add 0.1 g H2V3O8 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to obtain solution A;
[0042] Step 2) Add 0.2 g of VO2 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to prepare solution B;
[0043] Step 3) Place Liquid A and Liquid B in separate hydrothermal reactor chambers (total volume 60 ml). Seal the hydrothermal reactor and heat in an oven. Ensure that Liquid A and Liquid B do not come into contact during heating until the reaction temperature is reached.
[0044] Step 4) When the reaction temperature in step 3) rises to 200°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 200°C for 1 hour.
[0045] Step 5) The reactor was continuously stirred and cooled to room temperature, and black powder of the H2V3O8 / MXene / VO2 heterojunction material was obtained after filtration, washing, and drying.
[0046] Example 4
[0047] Step 1) Add 0.1 g H2V3O8 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to obtain solution A;
[0048] Step 2) Add 0.1 g of VO2 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to prepare solution B;
[0049] Step 3) Place Liquid A and Liquid B in separate hydrothermal reactor chambers (total volume 60 ml). Seal the hydrothermal reactor and heat in an oven. Ensure that Liquid A and Liquid B do not come into contact during heating until the reaction temperature is reached.
[0050] Step 4) When the reaction temperature in step 3) rises to 180°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 180°C for 1 hour.
[0051] Step 5) The reactor was continuously stirred and cooled to room temperature, and black powder of the H2V3O8 / MXene / VO2 heterojunction material was obtained after filtration, washing, and drying.
[0052] Example 5
[0053] Step 1) Add 0.1 g H2V3O8 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to obtain solution A;
[0054] Step 2) Add 0.1 g of VO2 / MXene to 10 mL of aqueous solution and ultrasonicate for 10 min to prepare solution B;
[0055] Step 3) Place Liquid A and Liquid B in separate hydrothermal reactor chambers (total volume 60 ml). Seal the hydrothermal reactor and heat in an oven. Ensure that Liquid A and Liquid B do not come into contact during heating until the reaction temperature is reached.
[0056] Step 4) When the reaction temperature in step 3) rises to 220°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 220°C for 1 hour.
[0057] Step 5) The reactor was continuously stirred and cooled to room temperature, and black powder of the H2V3O8 / MXene / VO2 heterojunction material was obtained after filtration, washing, and drying.
[0058] Comparative Example 1
[0059] Step 1) Prepare 12 mL of 2.4 mol L -1 The V2O5 aqueous solution is used as liquid A;
[0060] Step 2) Prepare 12 mL of 0.01 mol L -1 Glucose solution was used as solution B, and 0.01 g MXene (0.83 g L -1 ) was added to solution B and ultrasonicated for 1 h;
[0061] Step 3) Place Solution A and Solution B in separate hydrothermal reactors (total volume 60 ml), seal the reactor, and heat in an oven. Ensure that Solution A and Solution B do not come into contact during heating until the reaction temperature is reached.
[0062] Step 4) When the reaction temperature in step 3) rises to 240°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 240°C for 1 hour.
[0063] Step 5) The reactor was continuously stirred and cooled to room temperature, and H2V3O8 / MXene black powder was obtained after filtration, washing, and drying.
[0064] Comparative Example 2
[0065] Step 1) Prepare 12 mL of 2.4 mol L -1 The V2O5 aqueous solution is used as liquid A;
[0066] Step 2) Prepare 12 mL of 0.01 mol L -1 Glucose solution was used as solution B, and 0.03 g MXene (1.25 g L -1 ) was added to solution B and ultrasonicated for 1 h;
[0067] Step 3) Place Solution A and Solution B in separate hydrothermal reactors (total volume 60 ml), seal the reactor, and heat in an oven. Ensure that Solution A and Solution B do not come into contact during heating until the reaction temperature is reached.
[0068] Step 4) When the reaction temperature in step 3) rises to 240°C, the hydrothermal reactor is rotated to mix liquid A and liquid B. The reactor is kept rotating and the reaction is carried out at 240°C for 1 hour.
[0069] Step 5) The reactor was continuously stirred and cooled to room temperature, and VO2 / MXene black powder was obtained after filtration, washing, and drying.
[0070] Table 1 Test results
[0071]
[0072]
[0073] As shown in Table 1, when the addition amount of H2V3O8 / MXene is 0.1g, the addition amount of VO2 / MXene is 0.1g, and the hydrothermal reaction temperature is 200℃, the material -1 The specific capacity at a current density of 457 mAh g -1 .
[0074] Among them, the H2V3O8 / MXene / VO2 electrodes prepared in Examples 1-5, the H2V3O8 / MXene electrodes prepared in Comparative Example 1, and the VO2 / MXene electrodes prepared in Comparative Example 2 were heated to 0.1Ag. -1 The cycling performance diagram at the current density is shown in Figure 4-6 As shown. Figure 6 As shown, the H2V3O8 / MXene / VO2 heterojunction electrode (457mAh g -1 ) has a significantly higher cycling performance than that of the single H2V3O8 / MXene electrode (381mAh g -1 ) and VO2 / MXene electrode (312mAh g-1 The interaction between the multiphases of the heterojunction material enhances structural stability. Furthermore, the successful construction of the heterojunction enables charge redistribution at the interface, and the formation of a built-in electric field accelerates ion diffusion dynamics and induces more active sites.
[0075] Depend on Figure 7 It can be seen that the peak of the (200) crystal plane at 10.6° represents H2V3O8 / MXene. During the discharge process, the peak shifted significantly to the right, the lattice shrank, the volume decreased, and gradually recovered during the charging process; while the peak of the (110) crystal plane at 25.3° represents VO2 / MXene. During the discharge process, the peak shifted to the left, the lattice expanded, the volume increased, and gradually recovered during charging. The schematic diagram is shown in FIG. Figure 8 As shown in the figure, the two materials exhibit opposite volume changes during the different charge and discharge phases. Therefore, combining the two significantly mitigates the volume expansion of the electrode material during charge and discharge, effectively improving the material's expansion resistance. Consequently, when used as the positive electrode in zinc-ion batteries, it exhibits excellent electrochemical performance.
Claims
1. An electrode material having excellent expansion resistance, characterized in that: It is a H2V3O8 / MXene / VO2 heterojunction material. During the discharge process, the volume of H2V3O8 / MXene shrinks and the volume of VO2 / MXene expands; during the charging process, the volume of H2V3O8 / MXene expands and the volume of VO2 / MXene shrinks.
2. The positive electrode material with excellent expansion resistance according to claim 1, characterized in that: Nanorod-shaped H2V3O8 / MXene and VO2 / MXene are evenly distributed on the surface of MXene nanosheets, forming H2V3O8 / MXene / VO2 heterojunction materials.
3. A method for preparing an electrode material having excellent expansion resistance according to claim 1 or 2, characterized in that: The following steps are involved: (1) preparing H2V3O8 / MXene aqueous solution as liquid A and VO2 / MXene aqueous solution as liquid B; (2) placing liquid A and liquid B in a hydrothermal reactor with different reaction chambers and heating them; (3) When the temperature reaches the reaction temperature, the hydrothermal reactor is rotated to mix liquid A and liquid B. During the reaction, the reactor is always in a rotating state, and the target material is prepared after the reaction.
4. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: During the heating process, ensure that liquid A and liquid B do not come into contact, and mix the samples when the temperature rises to the reaction temperature.
5. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: In step (1), the concentration of the H2V3O8 / MXene aqueous solution is 0.01-0.05 g / mL.
6. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: In step (2), the concentration of the VO2 / MXene aqueous solution is 0.01 to 0.05 g / mL.
7. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: In step (3), the reaction temperature is 180-240° C. and the reaction time is 1-3 h.
8. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: In step (3), the rotation speed is controlled at 10 to 15 rpm.
9. The method for preparing an electrode material having excellent expansion resistance according to claim 3, characterized in that: After the reaction is completed, the reactor is continuously stirred and cooled to room temperature, and a black powder electrode material is obtained after filtration, washing and drying.
10. Use of the electrode material with excellent expansion resistance according to claim 1 or 2 as a positive electrode material in a zinc ion battery.
Citation Information
Patent Citations
Vanadium-based positive electrode material, preparation method thereof and zinc ion battery
CN117976882A
Polydopamine-coated Ti < 3 > C < 2 > T < x > at-H2V3O8 material with sandwich structure as well as preparation method and application thereof
CN118248472A
H4v3o8, a new vanadium(IV) oxide electroactive material for aqueous and non aqueous batteries
US20130157138A1
Electrodes containing conductive metal oxides
US5017446A
Vanadium oxide cathode active material and method of making same
US5340671A