Lithium battery silicon-based negative electrode material and preparation method thereof
By using silicon-carbon negative electrode materials and adding single-walled carbon nanotubes in lithium-ion batteries, the preparation process is optimized to solve the problem of silicon volume expansion, improve battery performance and cycle stability, extend battery life and reduce internal resistance.
Patent Information
- Application Number
- CN202411036139.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-08
AI Technical Summary
Silicon, the anode material for lithium-ion batteries, undergoes serious volume expansion during the lithium-ion embedding process, leading to structural cracks, instability of the interface between the electrode and the electrolyte, and rapid decline in battery performance, making it difficult to meet high energy density requirements.
Using silicon-carbon negative electrode material, by adding single-walled carbon nanotubes and optimizing the preparation process, including adjusting the stirring temperature and rotation speed, a carbon nanotube-coated silicon-carbon structure is prepared to limit volume expansion and improve stirring uniformity to create a loose and porous electrode structure. .
It significantly suppresses the volume expansion of the silicon-carbon anode, improves the cycle stability and performance of the battery, extends the battery life, reduces the internal resistance, and improves thermal management and safety.
Smart Images

Figure CN118748248A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to a lithium battery silicon-based negative electrode material and a preparation method thereof. Background Art
[0002] As portable electronic devices and electric vehicles are increasingly demanding batteries with higher energy density, lithium-ion batteries are facing major technical challenges as the main power source of choice. Among them, the selection of battery anode materials is particularly critical. Silicon and carbon composites have attracted much attention as anode materials due to their high theoretical capacity, but silicon undergoes significant volume expansion during lithium ion embedding, which may lead to structural fracture of the anode material, instability of the electrode-electrolyte interface, and rapid degradation of battery performance. Therefore, reducing the expansion rate of silicon-carbon anodes is a key technical challenge in realizing their commercial application.
[0003] Although traditional graphite negative electrode materials have good stability, their theoretical capacity is limited and it is difficult to meet the needs of future battery development. Silicon has a theoretical capacity of up to 4200 mAh / g, which is much higher than the 372 mAh / g of graphite, making silicon an ideal choice for negative electrode materials. However, the volume expansion of silicon during the charging and discharging process can exceed 300%. This drastic volume change can cause the pulverization of active materials and the destruction of the electrode structure, seriously affecting the cycle stability and service life of the battery. In addition, volume expansion can also lead to instability of the solid electrolyte interface (SEI), increase the internal resistance of the battery, and thus reduce the overall performance of the battery.
[0004] To this end, we propose a lithium battery silicon-based negative electrode material and a preparation method thereof to reduce the expansion rate of the silicon-carbon negative electrode. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings existing in the prior art. In order to achieve the above purpose, the present invention adopts the following technical solutions: A lithium battery silicon-based negative electrode material comprises the following components in weight percentage: 30.0% to 40.0% graphite, 5.0% to 10.0% silicon carbon, 0.2% to 2.0% single-walled carbon nanotubes, 0.1% to 0.5% dispersant, 0.1% to 0.5% conductive agent, 40.0% to 50.0% deionized water, 2.0% to 5.0% auxiliary solvent and 10.0% to 15.0% binder, the total weight of the above components mixed is 100%, and the mass ratio of the silicon carbon to the single-walled carbon nanotubes is 1:0.1 to 0.15.
[0006] Further preferably, the dispersant is one or more of polyvinyl pyrrolidone, polyacrylamide, polyvinyl alcohol, polyethylene glycol, polystyrene, sodium lauryl sulfate and sodium carboxymethyl cellulose.
[0007] Further preferably, the conductive agent is one or more of conductive carbon black, conductive graphite and carbon nanotubes.
[0008] Further preferably, the auxiliary solvent includes one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl propionate, propyl propionate, ethyl fluoroacetate, ethyl methyl fluorocarbonate, dimethyl fluorocarbonate, and propylene fluorocarbonate.
[0009] More preferably, the binder is any one of PVDF, CMC, PAA, LA133 and sodium alginate.
[0010] A method for preparing a lithium battery silicon-based negative electrode material comprises the following steps: Step 1: Put graphite, silicon carbon powder, carbon nanotubes, dispersant and conductive carbon black in a stirring tank, dry mix, and stir at 40°C to 60°C for 30 to 80 minutes; Step 2: introduce deionized water as the main solvent into a stirring tank, stir and knead, and stir at 40°C to 60°C for 30 to 80 minutes; Step 3: After stirring the mixture in step 2 evenly, add auxiliary solvent and binder, and then add deionized water, pre-stir, and stir at 40°C to 60°C for 10 to 30 minutes; Step 4: Stir for 220 to 280 minutes at a vacuum degree of -60 KPa and 40 to 60 ° C; Step 5: Apply the slurry obtained in step 4 onto the current collector and dry it in a high-temperature drying oven to form a negative electrode sheet for the battery.
[0011] Further preferably, in step 1, step 2 and step 3, the stirring speed is 30 to 80 rpm, without rotation.
[0012] Further preferably, in step 4, the stirring speed is 30-80 rpm, and the rotation speed is 3000-3500 rpm.
[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention explores the inhibitory effect of different single-walled carbon nanotube coating ratios on the silicon-based expansion rate and the impact on battery performance; it is determined that the optimal coating ratio of silicon-carbon to single-walled carbon nanotubes is 1:0.1-0.15. At this coating ratio, the inhibitory effect on the expansion rate is most significant, and at the same time, the electrical performance and cycle performance can be greatly improved.
[0014] On the one hand, the present invention can prepare a structure of carbon nanotubes encapsulating silicon carbon by adding single-walled carbon nanotubes to the preparation process of silicon-carbon negative electrode, thereby limiting the volume expansion of silicon carbon. On the other hand, by optimizing the preparation process, increasing the stirring speed and temperature, the silicon base and CNT are mixed more evenly, and at the same time, a loose porous electrode structure with higher porosity is manufactured, thereby reducing the volume expansion when lithium ions are embedded in the silicon base. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 : SEM image of silicon-carbon particles prepared in Comparative Example 1.
[0016] Figure 2 : SEM image of silicon-carbon particles prepared in Comparative Example 2.
[0017] Figure 3 : Comparative Example 2 prepares the Raman image of silicon carbon.
[0018] Figure 4 : Example 3 prepares the Raman image of silicon carbon.
[0019] Figure 5 : Comparative Example 2 prepares the dQ / dV diagram of silicon carbon.
[0020] Figure 6 : Example 3 Preparation of dQ / dV diagram of silicon carbon.
[0021] Figure 7 : Molecular structure model diagram of silicon-carbon embedded lithium.
[0022] Figure 8 : Molecular structure model diagram of lithium embedding after silicon-carbon coating.
[0023] Fig. 9 : Electronic band structure diagram of lithium-intercalated silicon-carbon.
[0024] Fig.10 : Electronic band structure diagram of lithium insertion after silicon-carbon-carbon coating. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0026] Reference Figure 1-Figure 10, a silicon-based negative electrode material for a lithium battery, the silicon-based negative electrode material comprising the following components by weight percentage: 30.0% to 40.0% graphite, 5.0% to 10.0% silicon carbon, 0.2% to 2.0% single-walled carbon nanotubes, 0.1% to 0.5% dispersant, 0.1% to 0.5% conductive agent, 40.0% to 50.0% deionized water, 2.0% to 5.0% auxiliary solvent and 10.0% to 15.0% binder, the total weight of the above components mixed is 100%, and the mass ratio of the silicon carbon to the single-walled carbon nanotubes is 1:0.1 to 0.15.
[0027] The dispersant is one or more of polyvinyl pyrrolidone, polyacrylamide, polyvinyl alcohol, polyethylene glycol, polystyrene, sodium lauryl sulfate and sodium carboxymethyl cellulose.
[0028] The conductive agent is one or more of conductive carbon black, conductive graphite and carbon nanotubes.
[0029] The auxiliary solvent includes one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl propionate, propyl propionate, ethyl fluoroacetate, ethyl methyl fluorocarbonate, dimethyl fluorocarbonate, and propylene fluorocarbonate.
[0030] The binder is any one of PVDF, CMC, PAA, LA133 and sodium alginate.
[0031] A method for preparing a lithium battery silicon-based negative electrode material comprises the following steps: Step 1: Put graphite, silicon carbon powder, carbon nanotubes, dispersant and conductive carbon black in a stirring tank, dry mix them, and stir them at 40℃~60℃ for 30~80min; Step 2: Introduce deionized water as the main solvent into the stirring tank, stir and knead them, and stir them at 40℃~60℃ for 30~80min; Step 3: After stirring step 2 evenly, add auxiliary solvent and binder, then add deionized water, pre-stir, and stir at 40℃~60℃ for 10~30min; Step 4: Stir at a vacuum degree of -60KPa and 40℃~60℃ for 220~280min; Step 5: Apply the slurry obtained in step 4 to the current collector, and put it into a high-temperature drying oven for drying to make a negative electrode sheet of the battery.
[0032] In step 1, step 2 and step 3, the stirring speed is 30-80 rpm without rotation. In step 4, the stirring speed is 30-80 rpm and the rotation speed is 3000-3500 rpm.
[0033] In order to suppress the significant volume expansion of silicon in the lithium battery silicon-carbon negative electrode material during the lithium ion embedding process, this patent preferably raises the stirring temperature to 50°C, and adds single-walled carbon nanotubes to suppress the volume expansion of the silicon-carbon material, while improving battery performance. Suppressing volume expansion helps to improve structural stability, reduce irreversible capacity loss, and enhance battery cycle life. Reducing the internal resistance of lithium batteries helps to improve thermal management, reduce battery aging rate, and improve battery safety. It plays an important role in improving battery performance, extending battery life, ensuring battery safety, and reducing manufacturing and operating costs.
[0034] The application of lithium battery silicon-based negative electrode materials and preparation methods thereof are illustrated below through a number of specific embodiments.
[0035] Comparative Example 1 Step 1: Place 6 kg of graphite, 1 kg of silicon-carbon powder, 0.037 kg of dispersant (carboxymethyl cellulose), and 0.059 kg of conductive carbon black in a stirring tank, dry mix, and stir at 45 ° C for 60 min, with a revolution speed of 50 rpm and no rotation.
[0036] Step 2: Weigh 2.018 kg of deionized water as the main solvent, introduce it into a stirring tank, stir and knead it, stir it at 45°C for 60 min, and rotate it at a speed of 50 rpm without rotation.
[0037] Step 3: After stirring evenly in step 2, add weighed 0.368 kg of auxiliary solvent (ethylene carbonate) and 2.088 kg of binder (PPA), and then add 4.917 kg of main solvent deionized water, pre-stir, stir at 45°C for 15 minutes, revolution speed 50 rpm, no rotation.
[0038] Step 4: Then stir with full force at 45°C for 250 min, with an orbital speed of 50 rpm, a rotation speed of 3200 rpm, and a vacuum degree of -60 KPa.
[0039] Step 5: Apply the slurry obtained in step 4 onto the current collector and dry it in a high-temperature drying oven to form a negative electrode sheet for the battery; make the negative electrode sheet into a battery cell according to conventional methods, and perform performance and cycle tests.
[0040] Comparative Example 2 A lithium battery is prepared in the same manner as in Comparative Example 1, and preferably the stirring temperature in steps 1 to 3 is increased to 50°C. Example
[0041] A lithium battery was prepared in the same manner as in Comparative Example 2, preferably with 0.05 kg of single-walled carbon nanotubes added in step 1. Example
[0042] A lithium battery is prepared in the same manner as in Comparative Example 2, and preferably single-walled carbon nanotubes with a silicon-carbon mass ratio of 0.1 kg are added in step 1. Example
[0043] A lithium battery is prepared in the same manner as in Comparative Example 2, and preferably single-walled carbon nanotubes with a silicon-carbon mass ratio of 0.15 kg are added in step 1. Example
[0044] A lithium battery is prepared in the same manner as in Comparative Example 2, and preferably single-walled carbon nanotubes with a silicon-carbon mass ratio of 0.2 kg are added in step 1.
[0045] Performance Testing The silicon-carbon negative electrode materials prepared in the above comparative examples and embodiments were made into corresponding positive electrodes of batteries according to conventional methods, and relevant tests on the corresponding performance of the batteries were carried out. The test data are compared as follows: In order to explore the intrinsic mechanism of single-walled carbon nanotubes improving the performance of silicon-carbon materials, the molecular structure and electronic energy band calculations of silicon-carbon materials and silicon-carbon materials coated with carbon were performed by first-principles calculations. Molecular structure calculations show that after silicon-carbon carbon coating and lithium insertion, the interatomic bond lengths in the molecular structure are reduced to varying degrees compared to silicon-carbon lithium insertion, which shortens the a-axis and b-axis of the lattice, indicating that coating with single-walled CNTs is beneficial to inhibiting the volume expansion of silicon-carbon after lithium insertion. At the same time, coating with single-walled CNTs is beneficial to reducing the band gap value of the electronic energy band of silicon-carbon materials, reducing resistance and improving electronic conductivity.
[0046] The battery performance test shows that when the stirring temperature is increased from 45°C to the preferred 50°C, the battery internal resistance is reduced, and the cycle life and gram capacity are improved, indicating that the preferred process temperature of 50°C is beneficial to improving the battery performance of silicon-carbon composite single-walled carbon nanotubes. Figure 1 and Figure 2 It can be seen from the SEM image that after the stirring temperature is increased to 50°C, the number of small particles in the SEM image increases significantly, indicating that the stirring effect is better after the temperature is increased to 50°C; this is because the mixing effect of single-walled carbon nanotubes and silicon carbon is better after the stirring temperature is increased.
[0047] from Figure 3 (Raman image of silicon carbon prepared in Comparative Example 2 (no single-walled carbon nanotubes added)) and Figure 4(Raman image of silicon carbon prepared in Example 3 (adding 15% single-walled carbon nanotubes)) It can be seen that characteristic peaks appear at 1338 cm-1 and about 1600 cm-1, corresponding to atomic crystal defects and in-plane stretching vibrations of C atom sp2 hybridization, respectively. The ratio of the peak intensities of the two can characterize the degree of defect in the carbon layer of the material. The smaller the ratio, the higher the degree of graphitization of the carbon layer, corresponding to better conductivity. It can be seen that the ratio of the two characteristic peak intensities is significantly reduced after adding 15% single-walled carbon nanotubes, indicating better conductivity.
[0048] from Figure 5 and Figure 6 It can be seen that 0.45V corresponds to the phase transition point of crystalline silicon. A high peak value indicates a greater volume expansion of the material. After adding 15% single-walled carbon nanotubes, the peak value corresponding to 0.45V drops from 2.3443 mAh / V to 1.4820 mAh / V, indicating that the addition of 15% single-walled carbon nanotubes significantly inhibits the volume expansion of silicon-carbon.
[0049] from Figure 7 and Figure 8 It can be seen that the composite single-walled carbon nanotube can be regarded as a layer of carbon coating; after carbon coating, the volume of the silicon-carbon lithium-intercalated structure is compressed from 167.36Å3 to 69.16Å3, and the volume is significantly reduced. From the specific model of the molecular structure model, it is known that the interatomic bond length is reduced to varying degrees, and the length of the lattice a-axis and b-axis is significantly reduced, which makes the molecular volume significantly reduced. This shows that a layer of carbon coating on the composite single-walled carbon nanotube can inhibit the volume expansion after silicon-carbon lithium-intercalation.
[0050] from Fig. 9 and Fig.10 As can be seen in the figure, the band gap in the electronic energy band structure diagram can characterize the difficulty of electronic transition in the structure. The smaller the band gap, the smaller the resistance and the greater the electronic conductivity. After carbon coating, the electronic energy band gap drops from 0.99 eV to 0.44 eV. From the first principle calculation level, it is proved that the reduction of silicon carbon internal resistance after carbon coating is due to the reduction of electronic energy band gap, which helps to improve the conductivity of the material, reduce heat generation and improve battery performance.
[0051] Comparative Example 2 and Example 1 can prove that when the stirring temperature is the same at 50 degrees Celsius, adding 0.05 kg of single-walled carbon nanotubes is beneficial to improving battery performance. When the addition amount of single-walled carbon nanotubes continues to increase to 0.15 kg, the battery performance continues to be optimized. Figure 3 and Figure 4 The Raman graph proves that the addition of 0.15 kg of single-walled carbon nanotubes reduces the degree of carbon layer defects in the silicon-carbon material compared to no addition. The higher the degree of graphitization of the carbon layer, the better the conductivity. Figure 5 and Figure 6They are the dQ / dV diagrams of the silicon-carbon negative electrode prepared by Comparative Example 2 (no single-walled carbon nanotubes added) and Example 3 (0.15kg single-walled carbon nanotubes added). It can be seen from the figure that after adding 0.15kg single-walled carbon nanotubes, the peak value corresponding to 0.45V dropped from 2.3443 mAh / V to 1.4820 mAh / V. It shows that the addition of 0.15kg single-walled carbon nanotubes significantly inhibits the volume expansion of silicon-carbon. However, when the amount of single-walled carbon nanotubes continues to increase to 0.2kg, the internal resistance of the battery begins to increase and the cycle performance begins to deteriorate, indicating that the optimal composite amount of single-walled carbon nanotubes is 10%-15% of the silicon-carbon mass ratio.
[0052] The present invention explores the inhibitory effect of different single-walled carbon nanotube coating ratios on the silicon-based expansion rate and the impact on battery performance; it is determined that the optimal coating ratio of silicon-carbon to single-walled carbon nanotubes is 1:0.1-0.15. At this coating ratio, the inhibitory effect on the expansion rate is most significant, and at the same time, the electrical performance and cycle performance can be greatly improved.
[0053] On the one hand, the present invention can prepare a structure of carbon nanotubes encapsulating silicon carbon by adding single-walled carbon nanotubes to the preparation process of silicon-carbon negative electrode, thereby limiting the volume expansion of silicon carbon. On the other hand, by optimizing the preparation process, increasing the stirring speed and temperature, the silicon base and CNT are mixed more evenly, and at the same time, a loose porous electrode structure with higher porosity is manufactured, thereby reducing the volume expansion when lithium ions are embedded in the silicon base.
Claims
1. A lithium battery silicon-based negative electrode material, characterized in that: The silicon-based negative electrode material includes the following components in weight percentage: 30.0% to 40.0% graphite, 5.0% to 10.0% silicon carbon, 0.2% to 2.0% single-walled carbon nanotubes, 0.1% to 0.5% dispersant, 0.1% to 0.5% conductive agent, 40.0% to 50.0% deionized water, 2.0% to 5.0% auxiliary solvent and 10.0% to 15.0% binder. The total weight of the above components mixed is 100%, and the mass ratio of the silicon carbon to the single-walled carbon nanotubes is 1:0.1 to 0.
15.
2. The lithium battery silicon-based negative electrode material according to claim 1, characterized in that The dispersant is one or more of polyvinyl pyrrolidone, polyacrylamide, polyvinyl alcohol, polyethylene glycol, polystyrene, sodium lauryl sulfate and sodium carboxymethyl cellulose.
3. The lithium battery silicon-based negative electrode material according to claim 1, characterized in that: The conductive agent is one or more of conductive carbon black, conductive graphite and carbon nanotubes.
4. The lithium battery silicon-based negative electrode material according to claim 1, characterized in that: The auxiliary solvent includes one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl propionate, propyl propionate, ethyl fluoroacetate, ethyl fluoromethyl carbonate, dimethyl fluorocarbonate, and propylene fluorocarbonate.
5. The lithium battery silicon-based negative electrode material according to claim 1, characterized in that: The binder is any one of PVDF, CMC, PAA, LA133 and sodium alginate.
6. The method for preparing a silicon-based negative electrode material for a lithium battery according to any one of claims 1 to 5, wherein: The following steps are involved: Step 1: Place graphite, silicon carbon powder, carbon nanotubes, dispersant, and conductive carbon black in a mixing tank, dry mix, and stir at 40°C to 60°C for 30 to 80 minutes; Step 2: Deionized water is introduced into a stirring tank as the main solvent, and the mixture is stirred and kneaded at 40°C to 60°C for 30 to 80 minutes; Step 3: After stirring the mixture in step 2 evenly, add the auxiliary solvent and binder, then add deionized water, pre-stir, and stir at 40°C to 60°C for 10 to 30 minutes; Step 4: Stirring at a vacuum degree of -60 kPa and a temperature of 40°C to 60°C for 220 to 280 minutes; Step 5: Apply the slurry obtained in step 4 onto the current collector and place it in a high-temperature drying oven for drying to form the battery negative electrode.
7. The method for preparing a silicon-based negative electrode material for a lithium battery according to claim 6, wherein: In step 1, step 2, and step 3, the stirring speed is 30 to 80 rpm, without rotation.
8. The method for preparing a silicon-based negative electrode material for a lithium battery according to claim 6, wherein: In step 4, the stirring speed is 30-80 rpm, and the rotation speed is 3000-3500 rpm.
Citation Information
Cited By
Low-expansion low-impedance lithium ion battery negative electrode and preparation method thereof
CN119447180A