Negative active material, preparation method, secondary battery and electric device

By preparing negative active materials with specific phase distribution, the problems of hindered sodium ion diffusion and increased side reactions in sodium-ion batteries are solved, and efficient energy storage and cycle performance of sodium-ion batteries are achieved.

CN118748252APending Publication Date: 2024-10-08SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410765653.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Due to the large radius of sodium ions in sodium-ion batteries, diffusion in negative electrode materials such as graphite is blocked, which cannot meet the demand for sodium storage. Moreover, the uncertainty in the phase composition of the negative electrode materials leads to an increase in side reactions, which limits the large-scale application of sodium-ion batteries.

Method used

By preparing negative active materials with specific phase distribution, including the first phase and the second phase, adjusting the peak area ratio of its X-ray diffraction pattern, increasing the intercalation and extraction ability of sodium ions, reducing the degree of side reactions, and reducing the amount of side reactions through heat treatment Oxygen-containing functional groups optimize the pore structure to improve the first Coulombic efficiency of the battery.

Benefits of technology

It achieves the first excellent Coulombic efficiency and charging performance of sodium-ion batteries, reduces the degree of side reactions, and improves the cycle performance and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004893915030000161
    Figure BDA0004893915030000161
  • Figure BDA0004893915030000171
    Figure BDA0004893915030000171
  • Figure BDA0004893915030000172
    Figure BDA0004893915030000172
Patent Text Reader

Abstract

The invention discloses a negative electrode active material, a preparation method, a secondary battery and a power utilization device, the negative electrode active material comprises negative electrode active material particles, and the negative electrode active material particles comprise a first phase and a second phase; the X-ray diffraction pattern of the first phase has a first diffraction peak when 2 theta is in a range of 20.5-22 degrees, and the peak area of the first diffraction peak is S1; the X-ray diffraction pattern of the second phase has a second diffraction peak when 2 theta is 22-24.5 degrees, and the peak area of the second diffraction peak is S2; s1 / S0 is more than 40% and less than 60%, and S2 / S0 is more than 25% and less than 60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction pattern of the negative electrode active material particles in the range of 2 theta being 10-30 degrees. The negative electrode active material provided by the invention has specific phase distribution, can reduce the side reaction degree, and enables the secondary battery to have excellent first coulombic efficiency, high energy density and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a negative electrode active material, a preparation method, a secondary battery and an electrical device. Background Art

[0002] In sodium-ion batteries, the diffusion of sodium ions in negative electrode materials such as graphite is hindered due to the large radius of sodium ions, and the sodium storage demand cannot be met. Therefore, in order to improve the sodium storage capacity of negative electrode materials, the interlamellar spacing of negative electrode materials needs to be increased, but the interlamellar spacing is related to the phase composition of negative electrode materials. Due to the uncertainty of the phase composition of negative electrode materials, the degree of side reactions on the negative electrode increases, resulting in undesirable first coulomb efficiency, which limits the large-scale application of sodium-ion batteries. Summary of the invention

[0003] Purpose of the invention: The present application provides a negative electrode active material, a preparation method, a secondary battery and an electrical device, and improves the first coulombic efficiency of the secondary battery by adjusting the negative electrode active material with a suitable phase distribution.

[0004] Technical solution: A negative electrode active material of the present application includes negative electrode active material particles, wherein the negative electrode active material particles include a first phase and a second phase;

[0005] The X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S1;

[0006] The X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S2;

[0007] The negative electrode active material particles satisfy: 40%<S1 / S0<60%, and 25%<S2 / S0<60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction spectrum of the negative electrode active material particles within the range of 2θ of 10° to 30°.

[0008] In some embodiments, the negative electrode active material particles further include a third phase, the X-ray diffraction spectrum of the third phase has a third diffraction peak in the range of 2θ of 24.5° to 26.5°, and the peak area of ​​the third diffraction peak is S3;

[0009] The negative electrode active material particles further satisfy: 0<S3 / S0<15%.

[0010] In some embodiments, the negative electrode active material particles have oxygen-containing functional groups, and the oxygen-containing functional groups can escape from the negative electrode active material particles in the form of gas. The escaped gas has a maximum mass concentration of P0 ppm, satisfying: 0<P0≤20000.

[0011] In some embodiments, the oxygen-containing functional group includes at least one of a hydroxyl group, an aldehyde group, a carboxyl group, an ester group, an amide group, and a carbonyl group; and / or

[0012] The gas comprises carbon dioxide; and / or

[0013] Under an inert atmosphere, the negative electrode active material particles are heat-treated to allow the oxygen-containing functional groups to escape in the form of gas, wherein the heat treatment temperature is 800° C.

[0014] In some embodiments, the negative electrode active material particles have pores, and the pores include mesopores and micropores; the sum of the specific surface areas of the mesopores is B1 m 2 / g, the total specific surface area of ​​the micropores is B2 m 2 / g, the negative electrode active material particles further satisfy, 3≤B1+αB2≤15; wherein α is a correlation coefficient, and the range of α is 0.05 to 0.7.

[0015] In some embodiments, the negative electrode active material particles further satisfy at least one of the following characteristics:

[0016] a)3≤B1≤10;

[0017] b)3≤B2≤150.

[0018] In some embodiments, the correlation coefficient α further satisfies:

[0019] When B2<3, α is 0.7; or

[0020] When 3≤B2<5, α is 0.55; or

[0021] When 5≤B2<10, α is 0.35; or

[0022] When 10≤B2<50, α is 0.2; or

[0023] When 50≤B2<100, α is 0.1; or

[0024] When 100≤B2, α is 0.05.

[0025] In some embodiments, the present application also provides a method for preparing a negative electrode active material, comprising:

[0026] Taking the prepared raw material, performing the first carbonization, crushing and washing, and obtaining the first precursor;

[0027] Activating the first precursor to obtain a second precursor;

[0028] The second precursor is subjected to a second carbonization, screening and demagnetization to obtain a negative electrode active material;

[0029] Wherein, the negative electrode active material comprises negative electrode active material particles, and the negative electrode active material particles comprise a first phase and a second phase;

[0030] The X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S1;

[0031] The X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S2;

[0032] The negative electrode active material particles satisfy: 40%<S1 / S0<60%, and 25%<S2 / S0<60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction spectrum of the negative electrode active material particles within the range of 2θ of 10° to 30°.

[0033] In some embodiments, the preparation raw material includes at least one of biomass carbon, resin, asphalt, and coal; and / or

[0034] The treatment temperature of the first carbonization is 500-900° C., the treatment time of the first carbonization is 2-6 hours, the heating rate is 2-5° C. / min, and the treatment atmosphere is an inert atmosphere; and / or

[0035] The treatment temperature of the second carbonization is 1000-1400° C., the treatment time of the second carbonization is 5-15 hours, the heating rate is 10-50° C. / min, and the treatment atmosphere is an inert atmosphere.

[0036] In some embodiments, before the first carbonization step, the method further comprises:

[0037] Cross-linking the raw material under an oxidative atmosphere, wherein the raw material comprises asphalt;

[0038] The amount of the oxidizing atmosphere introduced is 100 to 150 L / (Kg·h) relative to the weight of the raw materials; and the cross-linking treatment is heated to 140°C at a rate of 10 to 15°C / min, then heated to 200°C to 300°C at a rate of 2 to 5°C / min, and kept warm for 1 to 5 hours.

[0039] In some embodiments, the present application also provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, a separator and an electrolyte; wherein the negative electrode plate comprises a negative electrode collector and a negative electrode material active layer arranged on the negative electrode collector, and the negative electrode material active layer comprises the negative electrode active material; or, the negative electrode material active layer comprises the negative electrode active material prepared by the preparation method.

[0040] In some embodiments, the present application further provides an electrical device, comprising the secondary battery, wherein the secondary battery is used to supply power to the electrical device.

[0041] Beneficial effects: Compared with the prior art, a negative electrode active material of the present application includes negative electrode active material particles, and the negative electrode active material particles include a first phase and a second phase; the X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S1; the X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S2; the negative electrode active material particles satisfy: 40%<S1 / S0<60%, and 25%<S2 / S0<60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction spectrum of the negative electrode active material particles in the range of 2θ of 10° to 30°. The negative electrode active material provided by the present application has a specific phase distribution, and both the first phase and the second phase can allow the insertion and extraction of sodium ions, which can reduce the degree of side reactions, and the battery containing the above-mentioned negative electrode active material has excellent first coulomb efficiency.

[0042] It can be understood that, compared with the prior art, the preparation method of the negative electrode active material, the secondary battery and the electrical device provided in the embodiments of the present application have all the technical features and beneficial effects of the above-mentioned negative electrode active materials, which will not be repeated here. DETAILED DESCRIPTION

[0043] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0044] In the description of this application, the meaning of "plurality" is two or more, unless otherwise specifically defined. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.

[0045] In the description of the present application, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the purpose of the process can be achieved. In addition, in this specification, the numerical range displayed using "to" indicates a range that includes the numerical values ​​recorded before and after the "to" as the minimum and maximum values, respectively. In addition, in this specification, regarding the term "layer", when observed in a plan view, in addition to the configuration of a shape formed on the entire surface, it also includes the configuration of a shape formed on a portion.

[0046] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application.

[0047] The applicant found that sodium-ion batteries have attracted widespread attention due to their abundant resources and low prices. However, the radius of sodium ions (0.113nm) is larger than that of lithium ions (0.076nm), making it difficult for graphite, the negative electrode material of lithium-ion batteries, to meet the sodium storage requirements. Hard carbon has a large interlayer spacing, which allows sodium ions to be embedded and diffused, making it the most potential negative electrode material for sodium-ion batteries. However, the interlayer spacing is related to the physical composition of the negative electrode material. Due to the uncertainty of the physical composition of the negative electrode material, the degree of side reactions on the negative electrode increases, resulting in undesirable first coulomb efficiency and cycle performance, which limits the large-scale application of sodium-ion batteries. Therefore, it is necessary to prepare a negative electrode active material with a suitable physical phase distribution to obtain a secondary battery with better performance.

[0048] An embodiment of the present application provides a negative electrode active material, including negative electrode active material particles, the negative electrode active material particles including a first phase and a second phase; the X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S1; the X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S2; the negative electrode active material particles satisfy: 40%<S1 / S0<60%, and 25%<S2 / S0<60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction spectrum of the negative electrode active material particles in the range of 2θ of 10° to 30°.

[0049] Among them, the first phase can be understood as a highly disordered phase, the d002 crystal plane spacing of the first phase measured in the X-ray diffraction spectrum is greater than 0.4nm, sodium ions can freely enter and exit it, and the first phase stores sodium by an adsorption mechanism; the second phase is a pseudo-graphite phase, the d002 crystal plane spacing of the second phase measured in the X-ray diffraction spectrum is greater than 0.36nm and less than 0.4nm, and the second phase stores sodium by an interlayer embedding mechanism; the diffraction peak area of ​​the first phase and the second phase is determined by the X-ray diffraction spectrum, and the distribution of the first phase and the second phase in the negative active material is further limited. Under this specific phase distribution, the first phase and the second phase constitute a diffusion channel for sodium ions inside the active material to adjust the structure and properties of the active material particles, thereby improving the initial efficiency and charging performance of the battery. In addition, since the first phase has more lattice defects, the increase in the degree of side reactions can be reduced in the range of 40%<S1 / S0<60%, but the second phase itself also affects the sodium storage performance of the negative electrode active material, so in the range of 25%<S2 / S0<60%, the impact on the charge and discharge performance of the battery is reduced. The phase distribution of the first phase and the second phase is interrelated and affects each other. The negative electrode active material with a specific phase distribution in the above range can obtain an electric device with excellent first efficiency.

[0050] Furthermore, the X-ray diffraction pattern is obtained through an X-ray diffraction experiment. The specific process includes: obtaining a sample containing the desired phase, usually in the form of powder or crystals. The sample should be fine-grained and have sufficient purity and crystal structure; using an X-ray diffraction instrument, such as an X-ray diffractometer or an X-ray diffractometer. The instrument needs to be appropriately adjusted according to the experimental requirements, including setting the angle range, selecting the appropriate X-ray wavelength, and adjusting the incident angle; placing the sample in the instrument so that it interacts with the X-rays to produce diffraction phenomena. By rotating the sample or the detector in the instrument, the diffraction intensity corresponding to different scattering angles (2θ) is recorded; the obtained diffraction data can be calculated and analyzed to obtain information about the structure and composition of the sample. Common analysis methods include calculating lattice constants, determining crystal morphology, identifying crystal structure and relative crystal content, etc.

[0051] In some embodiments, the negative electrode active material particles also include a third phase, the X-ray diffraction pattern of the third phase has a third diffraction peak in the range of 2θ of 24.5° to 26.5°, and the peak area of ​​the third diffraction peak is S3; the negative electrode active material particles further satisfy: 0<S3 / S0<15%.

[0052] Among them, the third phase can be understood as a graphite-like phase. The d002 crystal plane spacing of the third phase measured in the X-ray diffraction spectrum is less than 0.36nm. Sodium ions cannot be embedded in the third phase due to their large ionic radius. The third phase can prevent the solid phase diffusion of sodium ions in the material particles. When the distribution of the third phase meets the range of 0<S3 / S0<15%, the fast charging performance of the negative electrode active material can be further adjusted to ensure that the electrical device has better charging capacity and first efficiency under the specified requirements.

[0053] In some embodiments, the negative electrode active material powder XRD test parameter settings of this embodiment include: scanning range: 10-30°, scanning speed: 3° / min, step length: 0.01°, obtaining XRD curve, removing background, performing peak separation on the peaks between 10 and 30°, first phase peak position: 20.5°-22°, second phase peak position: 22°-24.5°, third phase peak position: 24.5-26.5. The peaks are integrated respectively, recorded as S1, S2, S3, and the total peak area is recorded as S0.

[0054] In some embodiments, the negative electrode active material particles have oxygen-containing functional groups.

[0055] In some embodiments, the oxygen-containing functional groups in the negative electrode active material particles can escape from the negative electrode active material particles in the form of gas, and the escaped gas has a maximum mass concentration of P0 ppm, satisfying: 0<P0≤20000.

[0056] In some embodiments, further, the escaping gas has a maximum mass concentration P0 ppm satisfying: 0<P0≤5000.

[0057] It should be noted that due to the low heat treatment temperature during the preparation of the negative electrode active material, the oxygen-containing functional groups cannot be completely removed, but the oxygen-containing functional groups have an irreversible adsorption effect on sodium ions, which will lead to a decrease in the initial efficiency of the battery. Therefore, when the maximum mass concentration P0 ppm satisfies the range of 0<P0≤20000, the adsorption effect of the oxygen-containing functional groups on sodium ions can be reduced, and the initial efficiency of the battery can be further improved.

[0058] In some embodiments, the oxygen-containing functional group includes at least one of a hydroxyl group, an aldehyde group, a carboxyl group, an ester group, an amide group, and a carbonyl group.

[0059] In some embodiments, the evolved gas includes carbon dioxide.

[0060] In some embodiments, the oxygen-containing functional groups remaining in the negative electrode active material can be characterized by subjecting it to heat treatment, specifically: under an inert atmosphere, the negative electrode active material particles are heat treated to allow the oxygen-containing functional groups to escape in the form of gas, wherein the heat treatment temperature is 800°C, the heating rate is 5°C / min, and the inert gas atmosphere includes nitrogen (N2), helium (He), argon (Ar), etc.

[0061] In some embodiments, the maximum mass concentration P0 ppm can be obtained by mass spectrometry detection.

[0062] In some embodiments, the negative electrode active material particles have pores, the pores include mesopores and micropores; the sum of the specific surface areas of the mesopores is B1 m 2 / g, the total specific surface area of ​​micropores is B2 m 2 / g, the negative electrode active material particles further satisfy, 3≤B1+αB2≤15; wherein α is a correlation coefficient, and the range of α is 0.05 to 0.7.

[0063] It should be noted that the pore distribution and specific surface area of ​​the pores on the surface of the negative electrode active material particles have a significant correlation with the first efficiency of the battery. The larger the specific surface area, the more active sodium is consumed to form the SEI film, and the lower the first efficiency of the battery; but if the specific surface area is too small and the electrochemical reaction area is too small, the fast charging performance of the electrochemical device will decrease. Therefore, when 3≤B1+αB2≤15 is satisfied, and the range of α is 0.05-0.7, it shows that the pores on the surface of the negative electrode active material particles have specific distribution requirements, which can further balance the first efficiency and fast charging performance of the battery, and obtain a secondary battery with excellent cycle performance and high energy density.

[0064] In some embodiments, the average pore size of the mesopores is 2-50 nm, and the average pore size of the micropores is less than 2 nm.

[0065] In some embodiments, the total specific surface area of ​​the mesopores is B1 m 2 / g further satisfies: 3≤B1≤10; for example, B1 can be 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, or any value or range between any two values. The specific method of obtaining B1 is: using a specific surface area analyzer, N2 multi-point BET test, temperature 77K, relative pressure P / P0 of 0.02, 0.03, 0.04, 0.05 and 0.06, and calculating to obtain B1.

[0066] In some embodiments, the total specific surface area of ​​the micropores is B2 m 2 / g further satisfies: 3≤B2≤150; for example, B2 can be 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, 20m 2 / g, 30m 2 / g, 40m 2 / g, 50m 2 / g, 60m 2 / g, 70m 2 / g, 80m 2 / g, 90m 2 / g、100m 2 / g, 110m 2 / g, 120m 2 / g, 130m 2 / g, 140m 2 / g, 150m 2 / g is any value or the range between any two values. The specific method of obtaining B2 is: using a specific surface area analyzer, CO2 adsorption test, temperature 273K, relative pressure P / P0 between 0 and 0.03, randomly selecting 40 points, and processing with a DFT model to obtain B2.

[0067] In some embodiments, the correlation coefficient α is related to the total specific surface area of ​​the micropores B2, specifically: when B2<3, α is 0.7; when 3≤B2<5, α is 0.55; when 5≤B2<10, α is 0.35; when 10≤B2<50, α is 0.2; when 50≤B2<100, α is 0.1; when 100≤B2, α is 0.05. The correlation coefficient α determines the distribution state and proportion of micropores on the surface of the negative electrode active material particles, and directly affects the specific surface area of ​​the negative electrode active material particles. When the correlation coefficient α satisfies the range of 0.05 to 0.7, more active sites can be provided for electrochemical reactions, which helps to improve the reaction rate and capacity of the battery.

[0068] In some embodiments, the gram capacity of the negative electrode active material is 250 to 360 mAh; for example, it can be any one of 250 mAh, 260 mAh, 270 mAh, 280 mAh, 290 mAh, 300 mAh, 310 mAh, 320 mAh, 330 mAh, 340 mAh, 350 mAh, and 360 mAh, or a range between any two values. When the gram capacity of the negative electrode active material is within this range, the energy density of the secondary battery can be improved and a higher energy storage capacity can be maintained, and the electrical device can have better overall performance.

[0069] In some embodiments, the specific surface area of ​​the negative electrode active material is 3 to 10 m 2 / g, for example, it can be 3m 2 / g, 4m 2 / g, 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 When the specific surface area of ​​the negative electrode active material is within this range, the reaction degree of the battery can be improved, and the electrical device can have better comprehensive performance.

[0070] In some embodiments, the Dv50 of the negative electrode active material is 3 to 10 μm, wherein Dv50 μm is the particle size corresponding to when the cumulative volume percentage of the negative electrode active material reaches 50%. Dv50 can be any one of 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, or a range between any two values. When the Dv50 of the negative electrode active material is within this range, the negative electrode active material has a better particle size distribution, and the battery has better overall performance.

[0071] In some embodiments, this embodiment further provides a method for preparing a negative electrode active material, comprising:

[0072] Taking the prepared raw material, performing the first carbonization, crushing and washing, and obtaining the first precursor;

[0073] Activating the first precursor to obtain a second precursor;

[0074] The negative electrode active material is obtained by carbonizing, screening and demagnetizing the second precursor for the second time.

[0075] In some embodiments, by performing the first carbonization and the second carbonization treatment respectively, a negative electrode active material with a specific phase distribution, number of oxygen-containing functional groups and specific surface area can be prepared, which can effectively improve the charging capacity of the material and reduce the degree of side reactions. The secondary battery containing the above-mentioned negative electrode active material has excellent cycle performance, high energy density and good fast charging performance.

[0076] In some embodiments, the raw material is selected from at least one of biomass carbon, resin, asphalt, and coal.

[0077] In some embodiments, the activation process includes an acid-base etching method, a template method, or a gas etching method.

[0078] In some embodiments, the treatment temperature of the first carbonization is 500-900° C., the treatment time of the first carbonization is 2-6 hours, the heating rate is 2-5° C. / min, and the treatment atmosphere is an inert atmosphere, such as nitrogen or argon.

[0079] In some embodiments, the second carbonization treatment temperature is 1000-1400° C., the second carbonization treatment time is 5-15 h, the heating rate is 10-50° C. / min, and the treatment atmosphere is an inert atmosphere, such as nitrogen or argon.

[0080] In some embodiments, before the first carbonization step, the process further includes: cross-linking the raw material under an oxidizing atmosphere, wherein the raw material includes asphalt; wherein the amount of the oxidizing atmosphere introduced is 100-150 L / (Kg·h) relative to the weight of the raw material; and the cross-linking process is heated to 140°C at a rate of 10-15°C / min, then heated to 200-300°C at a rate of 2-5°C / min, and kept warm for 1-5 hours. The oxidizing atmosphere includes air, etc.

[0081] In some embodiments, the amount of oxidizing atmosphere introduced can be any value of 100 L / (Kg·h), 110 L / (Kg·h), 120 L / (Kg·h), 130 L / (Kg·h), 140 L / (Kg·h), 150 L / (Kg·h), or a range between any two values.

[0082] It should be noted that the phase structure can be adjusted by oxidative cross-linking treatment and high-temperature treatment of the second carbonization; specifically, the higher the degree of cross-linking, the more difficult it is for the molecules to stack into a layered structure at high temperature, and the higher the proportion of the first phase; or, the lower the second carbonization temperature, the higher the proportion of the first phase. Of course, a coating step can also be added, gas phase, solid phase or liquid phase, and coating can adjust the specific surface area of ​​the material, but because the coating layer content is usually small, it has little effect on the distribution of the phase.

[0083] In some embodiments, the present application also provides a secondary battery, including a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte in the secondary battery are further supplemented as follows:

[0084] Positive electrode

[0085] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.

[0086] In some embodiments, the positive electrode active material layer can be one or more layers. Each layer of the multi-layer positive electrode active material can contain the same or different positive electrode active materials. The positive electrode active material is any substance that can reversibly intercalate and deintercalate active ions.

[0087] The positive electrode sheet is a single-sided sheet or a double-sided sheet. When the positive electrode sheet is a single-sided sheet, the positive electrode active material layer is arranged on one surface of the negative electrode current collector. When the positive electrode sheet is a double-sided sheet, the positive electrode active material layer is arranged on both surfaces of the positive electrode current collector. The positive electrode sheet may also have a single-sided positive electrode sheet area and a double-sided positive electrode sheet area at the same time. When the positive electrode sheet has a single-sided positive electrode sheet area and a double-sided positive electrode sheet area at the same time, the thickness of the positive electrode sheet is the thickness of the double-sided positive electrode sheet area.

[0088] In some embodiments, the positive electrode active material comprises one or more of a layered transition metal oxide, a polyanion compound, and a Prussian blue analog.

[0089] In some embodiments, the positive electrode active material comprises a doping element and / or a coating element. There is no particular requirement for the doping element and / or the coating element, as long as the positive electrode active material can be made more stable.

[0090] In addition, the positive electrode active material layer further includes a positive electrode conductor and a positive electrode binder.

[0091] In some embodiments, the type of positive electrode conductive agent is not limited, and any known conductive agent can be used. Examples of positive electrode conductive agents may include but are not limited to acetylene black, carbon black, carbon nanotubes, graphene, etc. The above positive electrode conductive agents can be used alone or in any combination.

[0092] In some embodiments, the type of positive electrode binder used in the manufacture of the positive electrode active material layer is not particularly limited. In the case of the coating method, as long as it is a material that is soluble or dispersible in the liquid medium used in the manufacture of the electrode, it can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber and other rubber-like polymers; styrene-butadiene-styrene block copolymers or their hydrides, ethylene-propylene-diene terpolymers (EPDM), styrene-ethylene-butadiene-ethylene copolymers, styrene-isoprene-styrene block copolymers or their hydrides and other thermoplastic elastomer-like polymers; syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, propylene-α-olefin copolymers and other soft resin-like polymers; polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene-ethylene copolymers and other fluorine-based polymers; polymer compositions having ionic conductivity of alkali metal ions, etc. The above positive electrode binders can be used alone or in any combination.

[0093] In some embodiments, the type of solvent used to form the positive electrode slurry is not limited, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the positive electrode conductor, and the positive electrode binder. Examples of solvents used to form positive electrode slurries may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.

[0094] There is no particular limitation on the type of positive electrode current collector, which can be any known material suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; carbon materials such as carbon cloth and carbon paper; and composite materials formed by polymers and metal layers. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0095] There is no particular limitation on the form of the positive electrode current collector. When the positive electrode current collector is a metal material, the form of the positive electrode current collector may include but is not limited to metal foil, metal cylinder, metal strip roll, metal plate, metal foil, metal plate mesh, stamped metal, foamed metal, etc. When the positive electrode current collector is a carbon material, the form of the positive electrode current collector may include but is not limited to carbon plate, carbon film, carbon cylinder, etc.

[0096] In some embodiments, the intermediate product obtained during the preparation of the positive electrode active material can also be crushed and sieved to obtain a positive electrode active material with an optimized particle size distribution and specific surface area. There is no particular restriction on the crushing method, which can be selected according to actual needs, such as using a particle crusher. The preparation method of the positive electrode active material of the present application is not limited to the above preparation method, as long as the formed positive electrode active material has the characteristics shown in the present application.

[0097] In some embodiments, the preparation process of the positive electrode sheet may include the steps of stirring, coating, drying, cold pressing, slitting and cutting. The preparation of the positive electrode sheet includes: dispersing the positive electrode active material, the positive electrode conductive agent and the positive electrode binder in N-methylpyrrolidone (NMP) in a certain proportion, coating the obtained slurry on aluminum foil, drying, cold pressing and slitting to obtain the positive electrode sheet.

[0098] Negative electrode

[0099] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on at least one surface of the negative electrode current collector, the negative electrode active material layer contains a negative electrode active material, the negative electrode active material includes negative electrode active material particles, the negative electrode active material particles include a first phase and a second phase, the X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S1; the X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S2; the negative electrode active material particles satisfy: 40%<S1 / S0<60%, and 25%<S2 / S0<60%; wherein S0 is the sum of the peak areas of all diffraction peaks of the X-ray diffraction spectrum of the negative electrode active material particles in the range of 2θ of 10° to 30°.

[0100] The negative electrode sheet is a single-sided sheet or a double-sided sheet. When the negative electrode sheet is a single-sided sheet, the negative electrode active material layer is arranged on one surface of the negative electrode current collector. When the negative electrode sheet is a double-sided sheet, the negative electrode active material layer is arranged on both surfaces of the negative electrode current collector. The negative electrode sheet may also have a single-sided negative electrode sheet area and a double-sided negative electrode sheet area at the same time. When the negative electrode sheet has a single-sided negative electrode sheet area and a double-sided negative electrode sheet area at the same time, the thickness of the negative electrode sheet is the thickness of the double-sided negative electrode sheet area.

[0101] The type of negative electrode current collector is not particularly limited and can be selected according to actual needs. Preferably, aluminum foil or carbon-coated aluminum foil can be used.

[0102] Diaphragm

[0103] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. The type of separator is not particularly limited and can be selected according to actual needs. The separator can be a polypropylene film, a polyethylene film, a polyvinylidene fluoride film, a spandex film, an aramid film, or a multilayer composite film modified by a coating.

[0104] In some embodiments, the preparation of a secondary battery includes: stacking the positive electrode sheet, the separator, and the negative electrode sheet in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then winding them into a square bare cell, loading them into a battery casing, and then baking them at 65 to 95°C to remove water, injecting electrolyte, sealing, and obtaining a secondary battery after standing, hot and cold pressing, formation, clamping, capacity division and other processes.

[0105] In some embodiments, the secondary battery may include an outer package, which may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the secondary battery may also be a soft package, such as a bag-type soft package, and the material of the soft package may be plastic, such as one or more of polypropylene, polybutylene terephthalate, polybutylene succinate, etc.

[0106] In some embodiments, the shape of the secondary battery is not particularly limited, and it can be cylindrical, square, or any other shape.

[0107] Electrical devices

[0108] In some embodiments, the present application provides an electrical device, which includes the above-mentioned secondary battery. The electrical device can be an application device such as a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, and an electric tool. The vehicle can be a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, for example, a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and an electric tool for railways, for example, an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc. The embodiments of the present application do not impose any special restrictions on the above-mentioned devices.

[0109] The present invention has been tested many times, and some of the test results are now cited as references to further describe the invention in detail, and the following is a detailed description in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0110] Example 1

[0111] Asphalt with a softening point of 200°C is crushed into a powder with a Dv50 of 5μm, and air of 100L / (Kg·h) relative to the asphalt is introduced, and the temperature is raised to 140°C at a rate of 12°C / min, and then raised to 200°C at a rate of 3°C / min, and kept warm for 3h to complete the cross-linking treatment; then the raw material after the cross-linking treatment is subjected to the first carbonization treatment under nitrogen protection, the treatment temperature of the first carbonization is 700°C, the treatment time of the first carbonization is 4h, and the heating rate is 3°C / min; the particles after the first carbonization are crushed to a suitable particle size, and impurities are removed by washing to obtain a first precursor; the first precursor is activated by KOH, the mass ratio of KOH to the first precursor is 2:1, the activation temperature is 800°C, the activation time is 60min, and after activation, an appropriate amount of 1mol L -1 The mixture was stirred with dilute hydrochloric acid for 1 hour, washed with deionized water until neutral, and dried to obtain a second precursor; the second precursor was then subjected to a second carbonization treatment in a nitrogen atmosphere, and the temperature was increased to 1200°C at a heating rate of 30°C / min, and the mixture was kept warm for 6 hours. After screening and demagnetization, the negative electrode active material was obtained.

[0112] Example 2

[0113] Provided is a negative electrode active material, the preparation method is the same as that of Example 1, except that the KOH activation temperature is 700° C., the activation time is 30 min; and the treatment temperature of the second carbonization is 1100° C.

[0114] Example 3

[0115] Provided is a negative electrode active material, the preparation method is the same as that of Example 1, except that the KOH activation temperature is 600° C., the activation time is 30 min; and the treatment temperature of the second carbonization is 1000° C.

[0116] Example 4

[0117] A negative electrode active material is provided. The preparation method is the same as that in Example 1, except that 100 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at a rate of 12°C / min, and then raised to 200°C at a rate of 3°C / min, and kept warm for 2 hours to complete the cross-linking treatment; the KOH activation time is 30 minutes; and the second carbonization insulation time is 8 hours.

[0118] Example 5

[0119] A negative electrode active material is provided, and the preparation method is the same as that of Example 1, except that 120 L / (Kg·h) of air relative to asphalt is introduced, the temperature is raised to 140°C at 12°C / min, and then raised to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the KOH activation temperature is 600°C, and the activation time is 30 minutes; the treatment temperature of the second carbonization is 1100°C, the insulation time of the second carbonization is 5 hours, and the heating rate is 50°C / min.

[0120] Example 6

[0121] A negative electrode active material is provided, and the preparation method is the same as that of Example 5, except that 110 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at a rate of 12°C / min, and then to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the KOH activation temperature is 700°C, and the activation time is 60 minutes.

[0122] Example 7

[0123] A negative electrode active material is provided, and the preparation method is the same as that of Example 5, except that 100 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at 12°C / min, and then raised to 300°C at a rate of 3°C / min, and kept warm for 2 hours to complete the cross-linking treatment; the KOH activation temperature is 700°C, and the activation time is 30 minutes; the treatment temperature of the second carbonization is 1200°C, the insulation time of the second carbonization is 5 hours, and the heating rate is 50°C / min.

[0124] Example 8

[0125] A negative electrode active material is provided, and the preparation method is the same as that of Example 5, except that 150 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at a rate of 12°C / min, and then to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the KOH activation temperature is 800°C.

[0126] Example 9

[0127] A negative electrode active material is provided, and the preparation method is the same as that of Example 5, except that 140 L / (Kg·h) of air relative to asphalt is introduced, the temperature is raised to 140°C at 12°C / min, and then raised to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the KOH activation temperature is 800°C, and the activation time is 60 minutes; the treatment temperature of the second carbonization is 1300°C, the insulation time of the second carbonization is 10 hours, and the heating rate is 30°C / min.

[0128] Example 10

[0129] Provided is a negative electrode active material, the preparation method is the same as that of Example 9, except that the preparation raw material is biomass coconut shell, there is no air-introducing cross-linking step, and the KOH activation time is 30 minutes.

[0130] Embodiment 11

[0131] A negative electrode active material is provided, and the preparation method is the same as that of Example 9, except that 150 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is increased to 140°C at a rate of 12°C / min, and then increased to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the mass ratio of KOH to the first precursor is 3:1.

[0132] Example 12

[0133] A negative electrode active material is provided, and the preparation method is the same as that of Example 9, except that 150 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at 12°C / min, and then to 300°C at a rate of 3°C / min, and kept warm for 3 hours to complete the cross-linking treatment; the KOH activation time is 90 minutes; the insulation time for the second carbonization is 6 hours, and the heating rate is 50°C / min.

[0134] Embodiment 13

[0135] Provided is a negative electrode active material, the preparation method is the same as that of Example 9, except that the KOH activation temperature is 600° C., the activation time is 30 min; the insulation time for the second carbonization is 8 h, and the heating rate is 30° C. / min.

[0136] Embodiment 14

[0137] A negative electrode active material is provided, and the preparation method is the same as that of Example 9, except that the KOH activation temperature is 600°C.

[0138] Embodiment 15

[0139] Provided is a negative electrode active material, the preparation method is the same as that of Example 9, except that the KOH activation temperature is 700° C., the activation time is 30 min; the insulation time for the second carbonization is 8 h, and the heating rate is 10° C. / min.

[0140] Example 16

[0141] Provided is a negative electrode active material, the preparation method is the same as that of Example 9, except that the preparation raw material is phenolic resin, and there is no air-introducing cross-linking step; the KOH activation temperature is 600°C, the activation time is 30 min, and the mass ratio of KOH to the first precursor is 1:1; the insulation time for the second carbonization is 6 h, and the heating rate is 50°C / min.

[0142] Comparative Example 1

[0143] A negative electrode active material is provided. The specific preparation method is the same as that in Example 1, except that 150 L / (Kg·h) of air relative to asphalt is introduced, the temperature is raised to 140°C at 10°C / min, and then raised to 300°C at a rate of 3°C / min, and kept warm for 2 hours to complete the cross-linking treatment; the KOH activation time is 90 minutes; the treatment temperature of the second carbonization is 1500°C, the insulation time of the second carbonization is 10 hours, and the heating rate is 50°C / min.

[0144] Comparative Example 2

[0145] A negative electrode active material is provided. The specific preparation method is the same as that in Example 1, the KOH activation time is 30 minutes, the treatment temperature of the second carbonization is 900° C., and the insulation time of the second carbonization is 10 hours.

[0146] Comparative Example 3

[0147] A negative electrode active material is provided. The specific preparation method is the same as that in Example 1, except that 70 L / (Kg·h) of air relative to the asphalt is introduced, the temperature is raised to 140°C at a rate of 15°C / min, and then raised to 200°C at a rate of 3°C / min, and kept warm for 1 hour to complete the cross-linking treatment; the KOH activation temperature is 700°C; and the insulation time for the second carbonization is 10 hours.

[0148] The specific parameters of the phase distribution composition, the content of oxygen-containing functional groups and the pore distribution of the negative electrode active materials prepared in Examples 1 to 16 and Comparative Examples 1 to 3 are shown in Tables 1 and 2.

[0149] Table 1

[0150]

[0151]

[0152] Table 2

[0153]

[0154]

[0155] A secondary battery is prepared using the negative electrode active materials in Examples 1 to 16 and Comparative Examples 1 to 3. The specific preparation process includes:

[0156] (1) Preparation of positive electrode sheet

[0157] The positive electrode active material NaNi 0.33 Mn 0.33 Fe 0.33 O2, conductive agent carbon black, and binder PVDF are mixed in a mass ratio of 95:3:2, solvent NMP is added, and stirred under the action of a stirrer until the system is uniform to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, placed in an oven to dry, and rolled and cut to obtain positive electrode sheets.

[0158] (2) Preparation of negative electrode sheet

[0159] The negative electrode active material, conductive agent carbon black, thickener CMC, and binder SBR corresponding to each embodiment and comparative example were mixed in a mass ratio of 94.3:1.5:1.2:3, and deionized water was added as a solvent. The mixture was stirred in a stirrer until the system was uniform to obtain a negative electrode slurry. The negative electrode slurry was evenly coated on the negative electrode current collector aluminum foil, placed in an oven for drying, and rolled and cut to obtain negative electrode sheets.

[0160] (3) Preparation of electrolyte

[0161] Organic solvents ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate were mixed in a volume ratio of 1:1:1. In an argon atmosphere glove box with a water content of <10 ppm, fully dried sodium hexafluorophosphate was dissolved in the above organic solvents to a content of 1 mol / L, and mixed evenly to obtain an electrolyte.

[0162] (4) Preparation of secondary batteries

[0163] The positive electrode sheet, the separator (polyethylene), and the negative electrode sheet are wound in order to obtain a bare cell; the bare cell is placed in an outer packaging shell, vacuum dried, injected with electrolyte, left to stand, formed, shaped, and capacity divided to obtain a secondary battery.

[0164] The initial efficiency and charging capacity of the secondary batteries prepared in each embodiment and comparative example were tested. See Table 3 for specific test data.

[0165] Among them, first efficiency = first discharge capacity of full battery / first charge capacity;

[0166] The test of charging capacity is as follows: charge to 4.0V at xC, let stand for 5 minutes, discharge to 2.0V at 1C, cycle 10 times and disassemble the battery. If there is no sodium precipitation on the negative electrode, increase the charging current by 0.1C and repeat the above process until sodium precipitation occurs. The critical charging current for sodium precipitation is its charging capacity.

[0167] Table 3

[0168] First efficiency Charging Capacity Example 1 81.54% 0.8C Example 2 81.73% 0.7C Example 3 80.65% 1.1C Example 4 81.64% 0.7C Example 5 81.23% 1.8C Example 6 80.65% 1.5C Example 7 81.78% 1.2C Example 8 80.02% 2.0C Example 9 84.56% 1.3C Example 10 84.27% 1.5C Embodiment 11 84.02% 1.7C Example 12 83.78% 1.9C Embodiment 13 85.98% 1.5C Embodiment 14 86.13% 1.3C Embodiment 15 85.57% 1.8C Example 16 85.31% 2.0C Comparative Example 1 79.83% 1.0C Comparative Example 2 76.07% 2.0C Comparative Example 3 73.06% 0.1C

[0169] Referring to Table 1, Table 2 and Table 3, it can be seen from the results of Examples 1 to 4 that when the negative electrode active material of the secondary battery satisfies the range of 40%<S1 / S0<60% and 25%<S2 / S0<60%, the secondary battery has a higher first efficiency; compared with Comparative Examples 1 to 3, when the range of 40%<S1 / S0<60% and 25%<S2 / S0<60% is not satisfied, the first efficiency of the secondary battery decreases rapidly.

[0170] From the results of Examples 5 to 8, it can be seen that when the secondary battery simultaneously meets the ranges of 40%<S1 / S0<60%, 25%<S2 / S0<60% and 0<S3 / S0<15%, the initial efficiency of the secondary battery is further improved, and the secondary battery can also meet the charging requirements of 1.0C charging.

[0171] From the results of Examples 9 to 12, it can be seen that when the range of 0<P0≤20000 is met, the initial efficiency of the secondary battery can be further improved; from the results of Examples 13 to 16, it can be seen that when 3≤B1+αB2≤15 is met, the secondary battery can obtain higher initial efficiency and charging capacity.

[0172] The negative electrode active material, preparation method, secondary battery and electrical device provided in the embodiments of the present application are introduced in detail above. Specific examples are used in the present application to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solution and its core idea of ​​the present application. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A negative electrode active material, It is characterized in that The negative electrode active material particles include a first phase and a second phase; The X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S 1 ; The X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S 2 ; The negative electrode active material particles satisfy: 40%<S 1 / S 0 <60%, and 25%<S 2 / S 0 <60%; among them, S 0 It is the sum of the peak areas of all diffraction peaks in the X-ray diffraction spectrum of the negative electrode active material particles within the range of 2θ of 10° to 30°.

2. The negative electrode active material according to claim 1, It is characterized in that The negative electrode active material particles further include a third phase, the X-ray diffraction spectrum of the third phase has a third diffraction peak in the range of 2θ of 24.5° to 26.5°, and the peak area of ​​the third diffraction peak is S 3 ; The negative electrode active material particles further satisfy: 0<S 3 / S 0 <15%.

3. The negative electrode active material according to claim 2, It is characterized in that The negative electrode active material particles have oxygen-containing functional groups, and the oxygen-containing functional groups can escape from the negative electrode active material particles in the form of gas, and the escaped gas has a maximum mass concentration P 0 ppm, satisfying: 0<P 0 ≤20000.

4. The negative electrode active material according to claim 3, It is characterized in that The oxygen-containing functional group includes at least one of a hydroxyl group, an aldehyde group, a carboxyl group, an ester group, an amide group, and a carbonyl group; and / or The gas comprises carbon dioxide; and / or Under an inert atmosphere, the negative electrode active material particles are heat-treated to allow the oxygen-containing functional groups to escape in the form of gas, wherein the heat treatment temperature is 800° C.

5. The negative electrode active material according to claim 2, It is characterized in that The negative electrode active material particles have pores, and the pores include mesopores and micropores; the total specific surface area of ​​the mesopores is B 1 m 2 / g, the total specific surface area of ​​the micropores is B 2 m 2 / g, the negative electrode active material particles further satisfy, 3≤B 1 +αB 2 ≤15; where α is the correlation coefficient and the range of α is 0.05 to 0.

7.

6. The negative electrode active material according to claim 5, It is characterized in that The negative electrode active material particles further satisfy at least one of the following characteristics: a)3≤B 1 ≤10; b)3≤B 2 ≤150。 7. The negative electrode active material according to claim 5, It is characterized in that The correlation coefficient α further satisfies: B 2 When <3, α is 0.7; or 3≤B 2 When <5, α is 0.55; or 5≤B 2 When <10, α is 0.35; or 10≤B 2 When <50, α is 0.2; or 50≤B 2 When <100, α is 0.1; or 100≤B 2 When , α is taken as 0.

05.

8. A method for preparing a negative electrode active material, It is characterized in that include: Taking the prepared raw material, performing the first carbonization, crushing and washing, and obtaining the first precursor; Activating the first precursor to obtain a second precursor; The second precursor is subjected to a second carbonization, screening, and demagnetization to obtain a negative electrode active material; Wherein, the negative electrode active material comprises negative electrode active material particles, and the negative electrode active material particles comprise a first phase and a second phase; The X-ray diffraction spectrum of the first phase has a first diffraction peak in the range of 2θ of 20.5° to 22°, and the peak area of ​​the first diffraction peak is S 1 ; The X-ray diffraction spectrum of the second phase has a second diffraction peak in the range of 2θ of 22° to 24.5°, and the peak area of ​​the second diffraction peak is S 2 ; The negative electrode active material particles satisfy: 40%<S 1 / S 0 <60%, and 25%<S 2 / S 0 <60%; among them, S 0 It is the sum of the peak areas of all diffraction peaks in the X-ray diffraction spectrum of the negative electrode active material particles within the range of 2θ of 10° to 30°.

9. The method for preparing the negative electrode active material according to claim 8, It is characterized in that The raw material for preparation includes at least one of biomass carbon, resin, asphalt and coal; and / or The treatment temperature of the first carbonization is 500-900° C., the treatment time of the first carbonization is 2-6 hours, the heating rate is 2-5° C. / min, and the treatment atmosphere is an inert atmosphere; and / or The treatment temperature of the second carbonization is 1000-1400° C., the treatment time of the second carbonization is 5-15 hours, the heating rate is 10-50° C. / min, and the treatment atmosphere is an inert atmosphere.

10. The method for preparing the negative electrode active material according to claim 8, It is characterized in that Before the first carbonization step, it also includes: Cross-linking the raw material under an oxidative atmosphere, wherein the raw material comprises asphalt; The amount of the oxidizing atmosphere introduced is 100 to 150 L / (Kg·h) relative to the weight of the raw materials; and the cross-linking treatment is heated to 140°C at a rate of 10 to 15°C / min, then heated to 200°C to 300°C at a rate of 2 to 5°C / min, and kept warm for 1 to 5 hours.

11. A secondary battery, It is characterized in that It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode material active layer arranged on the negative electrode current collector, and the negative electrode material active layer comprises the negative electrode active material described in any one of claims 1 to 7; or, the negative electrode material active layer comprises the negative electrode active material prepared by the preparation method described in any one of claims 8 to 10.

12. An electrical device, It is characterized in that The secondary battery according to claim 11 is used to supply power to the electrical device.

Citation Information

Cited By

  • Negative electrode active material and preparation method therefor, secondary battery, and electric device

    WO2025256250A1