Multilayer film structures for bundled shrink films comprising multimodal ethylene terpolymers and recycled LDPE
By using the layered film structure of multimodal ethylene terpolymer and recycled LDPE in the bundled shrink film, the contradiction between the mechanical properties and recycled material content of the bundled shrink film is solved, and good mechanical properties and shrinkage under high recycled material content are achieved. behavior, reducing material usage and lowering the CO2 footprint.
Patent Information
- Application Number
- CN202280091253.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-11-10
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-11-10
AI Technical Summary
While existing bundled shrink films improve packaging stability and use recycled material content, it is difficult to maintain good mechanical properties and shrinkage behavior, and the reduction in film thickness challenges the stability of packaging.
It adopts a layered film structure including a core layer and an outer layer. The core layer is composed of multimodal ethylene terpolymer and recycled LDPE, and the outer layer contains multimodal ethylene terpolymer. This combination improves the rigidity and toughness of the film. , reducing material volume and lowering CO2 footprint.
It is possible to maintain the good mechanical properties and shrinkage behavior of the bundled shrink film under high recycled material content, reduce the amount of material used, without affecting the performance of the film, and improve packaging stability and sustainability.
Smart Images

Figure CN118748964A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a layered film structure comprising a core layer and an outer layer, a method for producing a layered film structure by coextrusion of these layers, a collation shrink film comprising the layered film structure, and the use of the collation shrink film for wrapping articles. Background Art
[0002] Collation shrink film is a film structure that is wrapped around an object to be packaged and shrinks to hold the units within the object together. The basic principle of collation shrink is to wrap some items from the outside in a loose film "sleeve" and then pass the wrapped goods through a heated shrink tunnel / oven for collation shrink wrapping. The film collapses around multiple items and holds them in place. The most common use of these films is to package multiple containers (items), such as bottles or cans that may contain food, beverages, etc. Collation shrink film is wrapped around multiple containers, such as 6 beverages or 24 food cans, which are optionally held in a cardboard tray or liner, and shrinks around the containers.
[0003] Today, up to 5% to 10% of goods are wasted during transportation. Improving the stability of wrap-around packaging with improved collation shrink film structures will allow producers to reduce losses. With today’s challenges and the overall direction of reducing film thickness, the stability of packaging is further compromised.
[0004] Therefore, in order to be suitable for use as a collation shrink film, the film structure needs to have a specific combination of properties: First and foremost, the film structure must exhibit good shrink behavior in order to hold the wrapped goods tightly. In addition, a suitable film structure needs to have: good mechanical properties, such as high stiffness, especially with regard to weight reduction capabilities and packaging stability; and good tensile properties.
[0005] Furthermore, puncture resistance and tear resistance are among the most important properties of collation shrink films in order to provide adequate package stability and enable safe handling of the package.
[0006] A good visual appearance is also required to make the package stand out on the shelf, ie as perceived by the consumer at the point of sale.
[0007] Currently, low density polyethylene (LDPE) dominates the collateral film market segment with its good shrink behavior, especially in the transverse direction (TD). However, it is known that multimodal LLDPE shows significant advantages over LDPE when blended with other linear low density polyethylene and high density polyethylene components.
[0008] Therefore, the current collation shrink film solution is a film structure including LDPE and LLDPE and / or HDPE. LDPE is necessary to produce high shrinkage, while the LLDPE / HDPE component provides a combination of rigidity, toughness and bundling force (also known as cold shrink force).
[0009] For example, WO 2017 / 055174 discloses a collated shrink film based on a coextruded film structure comprising two layers A and B, each of which is made of a specific ethylene copolymer.
[0010] Due to the latest regulations and market demands, the industry has to incorporate a certain amount of polymer recycled materials in packaging films. Due to the origin, previous use and difficulty in handling and sorting of post-consumer recycled (PCR) materials, recycled materials usually have lower technical properties compared to virgin materials, limiting or preventing their use in many applications.
[0011] Furthermore, it is desirable to have as high a PCR content as possible in flexible packaging without increasing the film thickness, while maintaining the performance of the final target application as described above.
[0012] Therefore, the market needs more sustainable films, i.e., using less material, optimally using as much recycled material as possible, while still meeting packaging needs with collation shrink films. This process is also called downsizing.
[0013] WO 2020 / 207940 discloses a multilayer collation shrink film consisting of a core layer B) sandwiched between two outer layers A), wherein the two outer layers A) consist of: a1) 12 wt.-% to 18 wt.-% of a multimodal polymer of ethylene with at least two different comonomers selected from α-olefins having 4 to 10 carbon atoms; a2) the multimodal polymer of ethylene having a density between 910 kg / m 3 Up to 935kg / m 3 a3) a multimodal terpolymer of 12 wt.-% to 18 wt.-% ethylene and at least two α-olefin comonomers, wherein the density of the multimodal terpolymer is between 930 kg / m 3 Up to 940kg / m 3 and 64wt.-% to 76wt.-% of the original polymer as a LDPE homopolymer having a density of 905kg / m 3 Up to 940kg / m 3and MFR2 in the range of 0.1 g / 10min to 20 g / 10min; and the core layer B) consists of: b1) 65 wt.-% to 75 wt.-% of recycled LDPE, whose MFR2 is in the range of 0.1 g / 10min to 10 g / 10min and density is 910 kg / m 3 Up to 940kg / m 3 and 35wt.-% to 25wt.-% of a multimodal terpolymer of ethylene and at least two α-olefin comonomers, wherein the density of the multimodal terpolymer is 930kg / m 3 Up to 940kg / m 3 However, the mechanical properties of the membrane can still be improved. Summary of the invention
[0014] It is therefore an object of the present invention to provide film structures suitable for use as collation shrink films meeting the above requirements, in particular film structures with increased amounts of post-consumer recycled (PCR) material, good shrink behaviour, and at the same time excellent stiffness and toughness.
[0015] The present invention is based on the discovery that such a film structure for collated shrink films can be provided by a layered film structure comprising a core layer and two outer layers, wherein the core layer and at least one of the outer layers comprise a specifically selected ethylene terpolymer.
[0016] Thus, the present invention provides a layered film structure comprising a core layer C and outer layers E1 and E2, wherein the core layer C comprises a multimodal ethylene terpolymer (I) having at least one C4 to C5 poly(ethylene) copolymer and recycled LDPE. 12 α-olefins, having an MFR5 of 0.1 g / 10 min to 5 g / 10 min determined according to ISO 1133 and having a 3 Up to 0.940g / cm 3 The recycled LDPE has a density of 0.1 g / 10 min to 10 g / 10 min determined according to ISO 1133 and has a MFR2 of 910 kg / m 3 Up to 940kg / m 3 wherein the outer layer E1 and / or the outer layer E2 comprises a multimodal ethylene terpolymer (II) having an MFR2 of 0.5 g / 10 min to 10 g / 10 min determined according to ISO 1133 and having a density of 0.920 g / cm 3 Up to 0.935g / cm 3 density.
[0017] The combination of the core layer C having the above characteristics with the outer layers E1 and E2 achieves the above objectives. In particular, even with a high content of recycled LDPE, this combination allows the film structure to remain rigid and tough, so that when used as a collation shrink film packaging, the amount of material can be reduced, and thus the CO2 footprint can be reduced, but the performance of the film is not affected.
[0018] Typically, the multimodal ethylene terpolymer (I) is different from the multimodal ethylene terpolymer (II).
[0019] Even more preferably, in the layered film structure the multimodal ethylene terpolymer (I) is a bimodal terpolymer comprising or consisting of:
[0020] a) low molecular weight polymers, which are ethylene and C4 to C 12 A binary copolymer of an alpha-olefin; and
[0021] b) a high molecular weight polymer, if the low molecular weight polymer of a) is ethylene and C6 to C 12 The high molecular weight polymer is a binary copolymer of ethylene and 1-butene, or the high molecular weight polymer is a binary copolymer of ethylene, 1-butene and C6 to C 12 Terpolymers of α-olefins.
[0022] Such bimodal ethylene terpolymers are disclosed, for example, in WO 03 / 066698. For the definition of these ethylene terpolymers (such as the "peak" of the polymer) and the production method, see WO 03 / 066698. In addition, whether explicitly described herein or not, the density described in WO 03 / 066698 is between 0.934 and 0.940 g / cm 3 All embodiments and preferred embodiments of this ethylene terpolymer within the scope of are also preferred embodiments of the ethylene terpolymer (I) in the present application.
[0023] Preferably, the density of the terpolymer (I) is 0.935 g / cm 3 Up to 0.939g / cm 3 within the range.
[0024] Preferably, the C4 to C 12 The α-olefin is selected from the group consisting of 1-butene, 1-hexene, 4-methyl-1-pentene, 1-octene and 1-decene.
[0025] In addition, preferably, the C6 to C 12 The α-olefin is preferably selected from the group of 1-hexene, 4-methyl-1-pentene, 1-octene and 1-decene.
[0026] In another preferred embodiment of the present invention, the terpolymer (I) comprises or consists of: a) a low molecular weight homopolymer of ethylene; and b) ethylene, 1-butene and C6 to C 12 The high molecular weight terpolymer of α-olefin is preferably a high molecular weight terpolymer of ethylene, 1-butene and 1-hexene.
[0027] The weight average molecular weight of the terpolymer (I) is preferably between 190,000 g / mol and 400,000 g / mol, more preferably between 200,000 g / mol and 300,000 g / mol. The weight average molecular weight of the low molecular weight polymer part is preferably between 4,500 g / mol and 55,000 g / mol, more preferably between 5,000 g / mol and 50,000 g / mol, and the weight average molecular weight of the high molecular weight polymer is preferably between 450,000 g / mol and 1,000,000 g / mol, more preferably between 500,000 g / mol and 1,000,000 g / mol.
[0028] The terpolymer (I) preferably has a melt flow rate MFR5 of 0.6 to 4 g / 10 min, more preferably 0.7 to 3 g / 10 min.
[0029] The terpolymer (I) preferably has a melt flow rate MFR of 10 g / 10 min to 50 g / 10 min. 21 , more preferably having a melt flow rate MFR of 15 to 45 g / 10 min 21 .
[0030] The low molecular weight polymer part of the terpolymer (I) preferably has a melt index MFR2 of 200 to 800 g / 10 min, more preferably 300 to 600 g / 10 min.
[0031] The terpolymer (I) preferably comprises 30 to 60 wt.-% of the low molecular weight polymer fraction, more preferably 35 to 50 wt.-% of the low molecular weight polymer fraction and most preferably 38 to 45 wt.-% of the low molecular weight polymer fraction, the remainder preferably being the high molecular weight polymer fraction.
[0032] The total comonomer content in the total polymer is preferably from 1 mol-% to 7 mol-%, more preferably from 2 mol-% to 6 mol-%.
[0033] Preferably, in low molecular weight polymers, the comonomer content is from 0 mol-% to 2.5 mol-%, more preferably from 0 mol-% to 2 mol-%. In high molecular weight polymers, the comonomer content is preferably from 2.5 mol-% to 11 mol-%, more preferably from 3 mol-% to 10 mol-%.
[0034] In embodiments where the terpolymer (I) comprises or consists of a) a low molecular weight homopolymer of ethylene and b) a high molecular weight terpolymer of ethylene, 1-butene and 1-hexene, it is preferred that the 1-butene content in the final polymer is from 1.0 to 2.0% by weight and the 1-hexene content is from 4.0 to 6.0% by weight.
[0035] Preferably, the viscosity η of the terpolymer (I) measured at 0.05 rad / s is 10,000 to 65,000 Pa·s, more preferably 15,000 to 60,000 Pa·s, most preferably 20,000 to 55,000 Pa·s.
[0036] A preferred multimodal terpolymer (I) is Borshape available from Borealis TM FX1002.
[0037] FX1002 is a bimodal MDPE terpolymer. The low molecular weight fraction is an ethylene homopolymer with an MFR2 of 400 g / 10 min, which is preferably produced in a loop reactor. In the high molecular weight fraction, which is preferably produced in a gas phase reactor, ethylene is copolymerized with 1-butene and 1-hexene as comonomers. The density of the final resin is 937 kg / m 3 , MFR5 is 2g / 10min, and MFR 21 The molecular weight of FX1002 is 42 g / 10 min. The ratio (LMW / HMW) is 43 / 57. The Mw / Mn of FX1002 is about 12 (11 to 13). The content of 1-butene in the final polymer is 1.5% by weight, and the content of 1-hexene is 4.5% by weight. The viscosity η measured at 0.05 rad / m is 23000 (+ / - 3000) Pa·s.
[0038] In the present disclosure, the term "recycled low density ethylene polymer" refers to a recycled polymer material comprising at least 80 wt.-%, preferably at least 75 wt.-%, more preferably at least 90 wt.-% and most preferably at least 95 wt.-% of LDPE, based on the total weight of recycled low density ethylene polymer that has been recycled. Thus, "recycled low density ethylene polymer" may contain up to 20 wt.-%, preferably up to 15 wt.-%, more preferably up to 10 wt.-% and most preferably up to 5 wt.-% of other polymer components (preferably recycled polymer components), such as LLDPE, MDPE and HDPE, based on the total weight of recycled low density ethylene polymer.
[0039] Recycled polymer materials are polymer materials recovered from post-consumer waste and / or industrial waste. Post-consumer waste refers to items that have completed at least their first use cycle (or life cycle), i.e. have served their first purpose, while industrial waste refers to manufacturing waste that does not normally reach consumers.
[0040] In contrast, the term "virgin" refers to an item that is before new material is produced and / or used for the first time and has not been recycled. In the absence of explicit reference to the source of a polymer, the polymer is a "virgin" polymer.
[0041] In one embodiment of the present invention, the recycled LDPE is derived from post-consumer waste.
[0042] Preferably, the recycled LDPE has an MFR2 determined according to ISO 1133 of 0.1 to 10 g / 10 min, more preferably 0.2 to 5 g / 10 min, still more preferably 0.25 to 1.0 g / 10 min, and most preferably 0.3 to 0.8 g / 10 min.
[0043] Preferably, the density of the recycled LDPE determined according to ISO 1183 is 910 kg / m 3 Up to 945kg / m 3 , preferably 910kg / m 3 Up to 940kg / m 3 , more preferably 915kg / m 3 Up to 935kg / m 3 , and most preferably 918 kg / m 3 Up to 930kg / m 3 .
[0044] Preferably, the melting point (secondary melt) of the recycled LDPE determined according to ISO 11357 is in the range of 105 to 130°C, preferably in the range of 108 to 125°C.
[0045] As recycled LDPE, the product NAV101 supplied by Ecoplast can be used.
[0046] The content of recycled LDPE present in the core layer composition is equal to or less than 80 wt.-%, based on the total weight of the core layer composition, preferably 62 wt.-% to 78 wt.-%, more preferably 65 wt.-% to 75 wt.-%, most preferably 68 wt.-% to 72 wt.-%.
[0047] The multimodal ethylene terpolymer (II) of the layered film structure of the present invention preferably comprises or consists of a multimodal polymer of ethylene and at least two different comonomers selected from α-olefins having 4 to 10 carbon atoms, the multimodal polymer having an MFR 21 The MFR / MFR2 ratio is 13 to 30 and the MWD is 5 or less.
[0048] Such multimodal ethylene terpolymers are disclosed, for example, in WO 2016 / 083208. For the definition of these ethylene terpolymers (such as the "modality" of the polymers) and the production methods, see WO 2016 / 083208. In addition, regardless of whether it is explicitly described herein, the density described in WO 2016 / 083208 is 0.910 g / cm 3 Up to 0.935g / cm 3 All embodiments and preferred embodiments of this ethylene terpolymer within the scope of are also preferred embodiments of the ethylene terpolymer (II) in the present application.
[0049] The MFR2 of the multimodal ethylene terpolymer (II) is preferably in the range of 0.5 to 2 g / 10 min, more preferably in the range of 0.8 to 1.6 g / 10 min.
[0050] Preferably, the multimodal ethylene terpolymer (II) has a density of 0.920 g / cm 3 Up to 0.933g / cm 3 , more preferably 0.923 g / cm 3 Up to 0.930g / cm 3 .
[0051] MFR of multimodal ethylene terpolymer (II) 21 The MFR / MFR2 ratio is preferably from 15 to 30, more preferably from 15 to 25.
[0052] The at least two α-olefin comonomers having 4 to 10 carbon atoms of the multimodal ethylene terpolymer (II) are preferably 1-butene and 1-hexene.
[0053] Preferably, the total amount of comonomers present in the multimodal ethylene terpolymer (II) is from 0.5 to 10 mol-%, preferably from 1.0 to 8 mol-%, more preferably from 1.0 to 5 mol-%, more preferably from 1.5 to 5.0 mol-%.
[0054] The multimodal ethylene terpolymer (II), which is preferably a bimodal terpolymer, preferably comprises or consists of an ethylene polymer fraction (A) and an ethylene polymer fraction (B), wherein the ethylene polymer fraction (A) has a higher MFR2 than the ethylene polymer fraction (B).
[0055] More preferably, the MFR2 of the ethylene polymer component (A) is 1 g / 10min to 50 g / 10min, preferably 1 g / 10min to 40 g / 10min, more preferably 1 g / 10min to 30 g / 10min, more preferably 2 g / 10min to 20 g / 10min, more preferably 2 g / 10min to 15 g / 10min, even more preferably 2 g / 10min to 10 g / 10min.
[0056] The ratio of the MFR2 of the ethylene polymer component (A) to the MFR2 of the final multimodal ethylene terpolymer (II) is from 2 to 50, preferably from 5 to 40, more preferably from 10 to 30, more preferably from 10 to 25 and still more preferably from 15 to 25.
[0057] Preferably, the ethylene polymer component (A) comprises a different comonomer than the ethylene polymer (B).
[0058] Preferably, the ethylene polymer fraction (A) has a smaller amount (mol%) of comonomers than the ethylene polymer fraction (B), more preferably the ratio of [amount (mol%) of α-olefin comonomers having 4 to 10 carbon atoms present in the ethylene polymer fraction (A)] to [amount (mol%) of at least two α-olefin comonomers having 4 to 10 carbon atoms in the final multimodal polymer of ethylene (a)] is from 0.2 to 0.6, preferably from 0.25 to 0.5.
[0059] Preferably, the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (A) is 1-butene, and the α-olefin comonomer having 4 to 10 carbon atoms of the ethylene polymer component (B) is 1-hexene.
[0060] Preferably, the density of ethylene polymer component (A) is different from, preferably higher than, the density of ethylene polymer component (B).
[0061] The density of the ethylene polymer component (A) is preferably 0.925 g / cm 3 Up to 0.950g / cm 3 , more preferably 0.930 g / cm 3 Up to 0.945g / cm 3 .
[0062] Preferably, the multimodal ethylene terpolymer (II) comprises: the ethylene polymer component (A) in an amount of 30 to 70 wt.-%, preferably 40 to 60 wt.-%, more preferably 35 to 50 wt.-%, more preferably 40 to 50 wt.-%; and the ethylene polymer component (B) in an amount of 70 to 30 wt.-%, preferably 60 to 40 wt.-%, more preferably 50 to 65 wt.-%, more preferably 50 to 60 wt.-%, based on the total amount of the multimodal terpolymer (II) (100 wt.-%).
[0063] Most preferably, the multimodal ethylene terpolymer (II) consists of ethylene polymer component (A) and ethylene polymer component (B) as the only polymer components. Thus, the ratio between ethylene polymer component (A) and ethylene polymer component (B) is (30 to 70):(70 to 30), preferably (40 to 60):(60 to 40), more preferably (35 to 50):(65 to 50), more preferably (40 to 50):(50 to 60).
[0064] The preferred multimodal ethylene terpolymer (II) is Anteo® also commercially available from Borealis or Borouge having the properties required herein. TM , especially Anteo TM FK-2715.
[0065] Preferably, in the laminar film structure according to the present invention the core layer C comprises 20 wt.-% or more, more preferably 22 wt.-% or more, still more preferably 25 wt.-% or more of said multimodal ethylene terpolymer (I). Preferably, in the laminar film structure according to the present invention the core layer C comprises 38 wt.-% or less, more preferably 35 wt.-% or less, still more preferably 32 wt.-% or less of said multimodal ethylene terpolymer (I).
[0066] In one embodiment the core layer C consists of the multimodal ethylene terpolymer (I) as defined herein and recycled LDPE.
[0067] The outer layer E1 and the outer layer E2 of the layered film structure of the present invention can be made of the same polymer composition or different polymer compositions in any of the embodiments of the polymer composition used for layer E1 and / or layer E2 described herein. Preferably, E1 and E2 are made of the same polymer composition.
[0068] Preferably, outer layer El and / or outer layer E2 comprises 60 wt.-% or more, more preferably 65 wt.-% or more of said multimodal ethylene terpolymer (II).
[0069] Apart from the multimodal ethylene terpolymer (II) the outer layer El and / or the outer layer E2 may also comprise a low density polyethylene (LDPE).
[0070] Preferably, if LDPE is present in outer layer El and / or outer layer E2, it is used in an amount of 5 to 40 wt.-%, more preferably 10 to 35 wt.-% and still more preferably 15 to 30 wt.-%.
[0071] The density of the LDPE used in layer E1 and / or layer E2 is preferably 0.905 g / cm 3 Up to 0.945g / cm 3 , more preferably 0.915 g / cm 3 Up to 0.935g / cm 3 , even more preferably 0.918 g / cm 3 Up to 0.927g / cm 3 , and most preferably 0.919 g / cm 3 Up to 0.922g / cm 3 .
[0072] Preferably, the MFR2 of the LDPE used in layer E1 and / or layer E2 is from 0.05 to 10 g / 10 min, more preferably from 0.10 to 5 g / 10 min, still more preferably from 0.20 to 3 g / 10 min, and most preferably from 0.25 to 0.70 g / 10 min.
[0073] In one embodiment the outer layer El and / or the outer layer E2 consists of the multimodal ethylene terpolymer (II) as defined herein and LDPE.
[0074] The layered film structure according to the invention may consist of a core layer C and outer layers E1 and E2.
[0075] The thickness of the layered film structure of the present invention according to any one of the embodiments described herein is preferably 100 microns or less, more preferably 60 microns or less, and most preferably 50 microns or less. In addition, the thickness of the layered film structure of the present invention according to any one of the embodiments described herein is preferably 20 microns or more, more preferably 30 microns or more, and most preferably 40 microns or more.
[0076] The thickness of the core layer C in the layered film structure of the present invention is preferably 45% to 75% of the thickness of the total film structure, more preferably 50% to 70% of the total film thickness.
[0077] Preferably, the thickness of each of the outer layer E1 and / or the outer layer E2 is from 10% to 25%, preferably from 15% to 25% of the thickness of the total film structure.
[0078] In addition, preferably, the layered film structure of the present invention has an Elmendorf tear resistance in the transverse direction measured on a 45 μm test film of 150 N / mm or more, more preferably 160 N / mm or more, and most preferably 180 N / mm or more. Preferably, the layered film structure of the present invention has an Elmendorf tear resistance in the transverse direction measured on a 45 μm test film of 250 N / mm or less, more preferably 230 N / mm or less, and most preferably 200 N / mm or less.
[0079] Furthermore, preferably, the layered film structure of the present invention has an Elemdorf tear resistance in the machine direction of 10 N / mm or more, more preferably 15 N / mm or more, and most preferably 28 N / mm or more. Preferably, the layered film structure of the present invention has an Elemdorf tear resistance in the machine direction of 40 N / mm or less, more preferably 35 N / mm or less, and most preferably 32 N / mm or less, measured on a 45 μm test film.
[0080] In addition, preferably, the tensile modulus of the layered film structure of the present invention in the transverse direction measured on a 45 μm test film is 200 MPa or more, more preferably 300 MPa or more, and most preferably 400 MPa or more. Preferably, the tensile modulus of the layered film structure of the present invention in the transverse direction measured on a 45 μm test film is 800 MPa or less, more preferably 600 MPa or less, and most preferably 500 MPa or less.
[0081] In addition, preferably, the tensile modulus of the layered film structure of the present invention in the machine direction measured on a 45 μm test film is 150 MPa or more, more preferably 200 MPa or more, and most preferably 300 MPa or more. Preferably, the tensile modulus of the layered film structure of the present invention in the machine direction measured on a 45 μm test film is 600 MPa or less, more preferably 500 MPa or less, and most preferably 400 MPa or less.
[0082] Preferably, the layered film structure of the present invention has a dart drop impact (DDI) determined according to ASTM D1709 on a 45 μm test film of greater than 70 g, preferably greater than 80 g, and most preferably greater than 100 g. In addition, preferably, the layered film structure of the present invention has a dart drop impact (DDI) determined according to ASTM D1709 on a 45 μm test film of less than 250 g, preferably less than 200 g, and most preferably less than 150 g.
[0083] Furthermore, preferably, the shrinkage of the layered film structure according to the invention in oil at 140° C. measured in the machine direction on a 45 μm test film according to DIN 55543-4 is 75% or more, more preferably 80% or more. Preferably, the shrinkage of the layered film structure according to the invention in oil at 140° C. measured in the machine direction on a 45 μm test film according to DIN 55543-4 is 90% or less, more preferably 85% or less.
[0084] Furthermore, preferably, the shrinkage of the layered film structure according to the invention in oil at 140° C. measured in the transverse direction on a 45 μm test film according to DIN 55543-4 is 10% or more. Preferably, the shrinkage of the layered film structure according to the invention in oil at 140° C. measured in the transverse direction on a 45 μm test film according to DIN 55543-4 is 30% or less, preferably 25% or less.
[0085] The invention further relates to a method for producing a layered film structure according to any of the above-mentioned embodiments, wherein a plurality of layers of the film structure are coextruded.
[0086] The different polymer components in any layer of the film are usually intimately mixed before the layer is formed, for example using a twin-screw extruder, preferably a counter-rotating extruder. The blend is then converted into a coextruded film structure. Preferably, the blend is converted into a coextruded film structure in a blown film line.
[0087] In order to manufacture such a multilayer film according to the present invention, at least two polymer melts are usually simultaneously extruded (i.e., co-extruded) through a multi-channel tubular, annular or circular die to form a tube, which is blown-up, inflated and / or cooled with air (or a combination of gases) to form a film. The manufacture of blown films is a well-known process.
[0088] Blown coextrusion may be carried out at a temperature in the range of 160°C to 240°C and cooled by blowing gas (usually air) at a temperature of 10°C to 50°C to provide a frost line height of 1 to 8 times the die diameter.
[0089] The blow up ratio (BUR) should generally be in the range of 1.2-6, preferably in the range of 1.5-4.
[0090] The layered film structure of the present invention may also be subjected to a stretching step, wherein the film is stretched in the machine direction (MDO) after it has been produced.Stretching may be performed by any conventional technique using any conventional stretching apparatus known to those skilled in the art.
[0091] The present invention also relates to a collation shrink film comprising or consisting of a layered film structure according to any of the embodiments described herein, and to the use of the collation shrink film for wrapping articles. BRIEF DESCRIPTION OF THE DRAWINGS
[0092] In the following, the present invention will be further described by way of embodiments with reference to the accompanying drawings, which show:
[0093] Figure 1: Graphical representation of the values given in Table 3 for IE1, CE1 and CE2. DETAILED DESCRIPTION
[0094] Measurement and determination methods
[0095] Unless otherwise defined, the following term definitions and determination methods apply to the above general description as well as the following examples of the invention.
[0096] a) Measurement of melt flow rate (MFR)
[0097] The melt flow rate (MFR) is determined according to ISO 1133 and is expressed in g / 10 min. The higher the melt flow rate, the lower the viscosity of the polymer. The MFR of polyethylene is 190°C and 2.16 kg (MFR2), 5.00 kg (MFR5) or 21.6 kg (MFR 21 ) is determined under load.
[0098] The FRR (Flow Rate Ratio) is an indicator of molecular weight distribution and represents the ratio of flow rates under different loads.21 / 5 Indicates MFR 21 / MFR5 value.
[0099] b) Density
[0100] The density of the polymer is measured according to ISO 1183-1:2019 (method A) on compression molded specimens prepared according to EN ISO 1872-2 (February 2007) and is expressed in g / cm 3 Given.
[0101] c) Shrinkage
[0102] The shrink properties of the collated shrink films were tested in the machine and transverse directions using an oil bath at 140°C (according to DIN 55543-4).
[0103] d) Dart impact
[0104] Dart Drop Impact (DDI) was determined according to ASTM D1709 "Method A" on films having the indicated thickness and produced as described below in "Examples".
[0105] e) Mechanical properties
[0106] Tensile modulus
[0107] TD (Transverse Direction) and MD (Machine Direction) of the Films For the blown films of the inventive examples, the tensile modulus in the machine and transverse directions was determined according to ISO 527-3 on films with a thickness of 45 microns at a crosshead speed of 1 mm / min.
[0108] Relative tear resistance
[0109] The tear strength or tear resistance is measured using the ISO 6383 / 2 method. The force required to propagate a tear on a film sample is measured using a pendulum apparatus. The pendulum swings along an arc under gravity, tearing the sample from a pre-cut seam. One side of the sample is fixed by the pendulum and the other side is fixed by a fixed fixture. The tear strength or tear resistance is the force required to tear the sample. The relative tear resistance (N / mm) can be calculated by dividing the tear resistance by the thickness of the film. The film is produced as described below in the film preparation example. The tear strength or tear resistance is measured in the machine direction (MD) and / or the transverse direction (TD).
[0110] Example
[0111] Three layered film structures (one layered film structure according to the invention and two layered film structures according to comparative examples) were produced on an Alpine Hosokawa film line. All film structures were produced under the same processing conditions (BUR 3:1, throughput 180 kg / h, thickness 45 microns (50 microns for CE3), die gap 1.5 mm, die diameter 200 mm, low neck-height, internal bubble cooling). The thickness of the core layer was 31.5 μm, and the thickness of each outer layer was 6.75 μm.
[0112] The polymers used to make the layered film structures of the invention and comparative examples are given in Table 1 below.
[0113] Table 1:
[0114]
[0115] *MFR 190℃ / 5kg
[0116] The composition and structure of the produced layered films are given in Table 2. In Table 2, "E" represents an outer layer, and "C" represents a core layer. The outer layers of the produced films each had the same composition.
[0117] Table 2: Layer structure of the example
[0118]
[0119] *Inventive Example 1 of WO 2020 / 207940 A1
[0120] Table 3: Properties of layer structures
[0121] CE3 CE2 CE1 IE1 MD shrinkage, % 72 82 81 78 TD shrinkage, % 25 10.4 9.3 10.5 Drop dart impact (DDI), g nm 67 75 108 Elemdorf tear resistance on MD, N / mm nm 10 13 28 Elemdorf tear resistance on TD, N / mm nm 146 146 183 Film tensile modulus MD, MPa nm 316 316 301 Film tensile modulus TD, MPa nm 459 459 406
[0122] nm—not measured
[0123] As can be seen from Table 3 and Figure 1, the use of FX1002 allows the use of 70 wt.-% PCR in the core layer while maintaining the same level of shrinkage performance, while providing higher mechanical properties, especially higher dart drop impact. It can further be seen that the outer layer of the invention also brings beneficial machine dimensional shrinkage. Finally, as shown in comparison with CE3, the composition of the outer layer of the invention allows further downsizing of the film structure without sacrificing shrinkage performance.
Claims
1. A layered film structure comprising a core layer C and outer layers E1 and E2, wherein: The core layer C comprises a multimodal ethylene terpolymer (I) having at least one C4 to C5 polyol and recycled LDPE. 12 α-olefins, having an MFR5 of 0.1 g / 10 min to 5 g / 10 min determined according to ISO 1133 and having an MFR of 0.934 g / cm 3 Up to 0.940g / cm 3 The recycled LDPE has a density of 0.1 g / 10 min to 10 g / 10 min determined according to ISO 1133 and has a MFR2 of 910 kg / m 3 Up to 940kg / m 3 wherein the outer layer E1 and / or the outer layer E2 comprises a multimodal ethylene terpolymer (II) having an MFR2 of 0.5 g / 10 min to 10 g / 10 min determined according to ISO 1133 and having a density of 0.920 g / cm 3 Up to 0.935g / cm 3 density.
2. The layered membrane structure according to claim 1, wherein: The multimodal ethylene terpolymer (I) is a bimodal terpolymer comprising: a) low molecular weight polymers, which are ethylene and C4 to C 12 A binary copolymer of α-olefins, and b) a high molecular weight polymer, if the low molecular weight polymer of a) is ethylene and C6 to C 12 The high molecular weight polymer is a binary copolymer of ethylene and 1-butene, or the high molecular weight polymer is a binary copolymer of ethylene, 1-butene and C6 to C 12 Terpolymers of α-olefins.
3. A layered membrane structure according to any one of the preceding claims, wherein: The multimodal ethylene terpolymer (II) comprises a multimodal polymer of ethylene and at least two different comonomers selected from α-olefins having 4 to 10 carbon atoms, the MFR of the multimodal polymer of ethylene and at least two different comonomers being 21 The ratio of MFR / MFR2 is from 13 to 30 and the MWD is 5 or less.
4. A layered membrane structure according to any one of the preceding claims, wherein: The core layer C comprises 38 wt.-% or less of said multimodal ethylene terpolymer (I).
5. A layered membrane structure according to any one of the preceding claims, wherein: The outer layer El and / or the outer layer E2 comprises 60 wt.-% or more of said multimodal ethylene terpolymer (II).
6. A layered membrane structure according to any one of the preceding claims, wherein: The film structure has a thickness of 100 microns or less.
7. A layered membrane structure according to any one of the preceding claims, wherein: The outer layer E1 and the outer layer E2 have the same composition.
8. A layered membrane structure according to any one of the preceding claims, wherein: The layered film structure of the present invention has an Elemdorf tear resistance in the transverse direction measured according to ISO 6383 / 2 of 150 N / mm or more, preferably 160 N / mm or more, and most preferably 180 N / mm or more.
9. A layered membrane structure according to any one of the preceding claims, wherein: The layered film structure of the present invention has an Elemdorf tear resistance in the machine direction measured according to ISO 6383 / 2 of 10 N / mm or more, preferably 15 N / mm or more, and most preferably 28 N / mm or more.
10. A layered membrane structure according to any one of the preceding claims, wherein The layered film structure of the present invention has a tensile modulus in the machine direction measured according to ISO 527-3 on a 45 μm test film of 150 MPa or more, preferably 200 MPa or more, and most preferably 300 MPa or more.
11. A layered membrane structure according to any one of the preceding claims, wherein The layered film structure of the present invention has a Dart Drop Impact (DDI) determined according to ASTM D1709 on a 45 μm test film of greater than 70 g, preferably greater than 80 g, and most preferably greater than 100 g.
12. A layered membrane structure according to any one of the preceding claims, wherein The shrinkage of the film structure in the machine direction and in oil at 140° C., determined according to ISO 55543-4 on a 45 μm test film, is 75% or more.
13. A method for producing a layered membrane structure according to any one of the preceding claims, wherein: The multiple layers of the film structure are coextruded.
14. A collated shrink film comprising or consisting of the layered film structure according to any one of claims 1 to 12.
15. Use of the collation shrink film according to claim 14 for wrapping articles.
Citation Information
Patent Citations
Polymer compositions, shrink films, and methods of making thereof
CN107108987A
Collation shrink film
CN113661062A
High shrink polyethylene films
CN1514853A
Machine direction oriented film with balanced properties at low stretch ratios
WO2016193186A1
Collation shrink film
WO2020207940A1