Composition of superabsorbent polymer and method for preparing same

By using additives such as aminoacetate chelating agents and cysteine ​​in superabsorbent polymers to form a surface cross-linked layer, the problem of odor and bacterial growth in products such as diapers is solved, and the deodorization and odor masking capabilities are improved. .

CN118749008APending Publication Date: 2024-10-08LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380019871.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2023-03-24
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult for existing superabsorbent polymers to effectively inhibit the odor and bacterial growth produced by urine in products such as diapers, resulting in insufficient deodorization and odor masking capabilities.

Method used

A superabsorbent polymer composition containing a base resin, a surface cross-linking layer, a aminoacetate chelating agent and cysteine ​​is used to cross-link with the surface cross-linking agent to form a cross-linked polymer, which is independently mixed during the preparation process Glycoacetate chelating agent and cysteine ​​to improve deodorizing ability and inhibit bacterial growth.

Benefits of technology

It can effectively inhibit odor production and bacterial growth without reducing the absorption performance, and significantly improve the deodorization ability and odor masking ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004974062950000201
    Figure BDA0004974062950000201
  • Figure BDA0004974062950000231
    Figure BDA0004974062950000231
Patent Text Reader

Abstract

The present invention relates to a composition of a superabsorbent polymer and a method for preparing the same, and more specifically, to a composition of a superabsorbent polymer and a method for preparing the same, which can effectively suppress odor generated by urine and the like when applied to a product such as a diaper by using a specific additive in combination, and which can effectively suppress odor generated by urine and the like when applied to a product such as a diaper and the like. The growth of bacteria in the wearing process of the product is inhibited, so that the deodorization capability and the smell masking capability are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0039062 filed on March 29, 2022, and Korean Patent Application No. 10-2023-0038011 filed on March 23, 2023, in the Korean Intellectual Property Office, the disclosures of which are incorporated herein by reference in their entirety.

[0003] The present invention relates to a superabsorbent polymer composition and a method for preparing the same. More specifically, the present invention relates to a superabsorbent polymer composition and a method for preparing the same, which can effectively suppress odors generated from urine and the like when applied to products such as diapers by using specific additives in combination, and suppress bacterial growth during product wearing, thereby improving deodorizing and odor masking capabilities. Background Art

[0004] Super absorbent polymer (SAP) is a synthetic polymer material that can absorb 500 to 1000 times its own weight of water. Depending on the company that developed it, it is also called super absorbent material (SAM), absorbent gel material (AGM), etc. Super absorbent polymers were first commercialized as sanitary products. At present, in addition to sanitary products such as disposable diapers for children, they are also widely used as soil water retention materials, water-stopping materials for civil engineering and construction, sheets for seedling cultivation, fresh-keeping preservatives in the field of food circulation, and dressing materials.

[0005] In most cases, such superabsorbent polymers are widely used in the field of sanitary products such as diapers or sanitary pads. In sanitary products, superabsorbent polymers are generally contained in pulp in a spread state. However, recently, in order to provide sanitary products such as diapers with a thinner thickness, diapers with reduced pulp content, or even pulp-free diapers that do not use pulp at all, are being actively developed.

[0006] Therefore, in the case of sanitary products with reduced pulp or pulp-free sanitary products, superabsorbent polymers are contained at a relatively high ratio, and such superabsorbent polymer particles are inevitably contained in multiple layers. Superabsorbent polymers should basically show high absorption performance and absorption speed so that all superabsorbent polymer particles contained in multiple layers can more effectively absorb liquids such as urine. In addition, the absorbed liquid should not leak even under external pressure, and in addition the superabsorbent polymer should have permeability so as to properly maintain the original shape even when it absorbs liquid and swells. Therefore, many studies are being conducted, such as surface cross-linking, to improve basic absorption and water retention capabilities.

[0007] Meanwhile, superabsorbent polymers can be used in sanitary products, and in this case, the after-use feeling may be deteriorated due to the smell of the absorbed liquid (such as human and pet excrement). In addition, as the wearing time passes, bacterial growth is accelerated, thereby generating odor.

[0008] Therefore, the demand for odor suppression as well as basic properties of superabsorbent polymers including absorption capacity and water retention capacity is gradually increasing. Therefore, it is necessary to prepare superabsorbent polymers having deodorizing ability and being able to effectively inhibit bacterial growth. Summary of the invention

[0009] Technical issues

[0010] The object of the present invention is to provide a super absorbent polymer composition and a method for preparing the same. More specifically, the object of the present invention is to provide a super absorbent polymer composition and a method for preparing the same, which can effectively suppress odors generated from urine and the like and inhibit bacterial growth when applied to products such as diapers by using specific additives in combination, thereby improving deodorizing ability and odor masking ability.

[0011] Technical Solution

[0012] In order to solve the above technical problems, the present invention provides a superabsorbent polymer composition, which comprises:

[0013] A superabsorbent polymer comprising a base resin and a surface crosslinked layer formed on a surface of the base resin, the base resin comprising a crosslinked polymer formed by crosslinking polymerization of an acrylic monomer having an at least partially neutralized acid group and an internal crosslinking agent, wherein the crosslinked polymer in the surface crosslinked layer is additionally crosslinked by a surface crosslinking agent;

[0014] Glycine chelating agents; and

[0015] Cysteine,

[0016] The aminoacetate (or salt) type chelating agent and cysteine ​​are each independently contained in the interior of the surface cross-linked layer or on the surface of the surface cross-linked layer.

[0017] The present invention also provides a method for preparing a superabsorbent polymer composition, which comprises the following steps:

[0018] In the presence of an internal crosslinking agent and a polymerization initiator, an acrylic monomer having an acid group that is at least partially neutralized is crosslinked and polymerized to form a hydrogel polymer (step 1);

[0019] preparing a base resin comprising a cross-linked polymer obtained by drying and grinding the hydrogel polymer (step 2);

[0020] mixing a surface cross-linking composition with the base resin to prepare a mixture (step 3); and

[0021] heat-treating the mixture to prepare a super absorbent polymer, wherein a surface cross-linked layer is formed on the surface of the base resin (step 4),

[0022] Wherein, in at least one of steps 2 to 4 and the steps before and after these steps, the aminoacetate (or salt) type chelating agent and cysteine ​​are mixed independently.

[0023] Beneficial Effects

[0024] As described above, the present invention is characterized by providing a super absorbent polymer composition having excellent deodorizing ability by using a specific additive in combination with a super absorbent polymer and inhibiting bacterial growth to inhibit generation of additional odor, and a method for preparing the same. DETAILED DESCRIPTION

[0025] The terms used herein are for explaining particular embodiments only and are not intended to limit the present invention.

[0026] Unless the context clearly indicates otherwise, a singular expression includes its plural expression. Throughout the specification, the terms "comprising", "equipped with", or "having" and the like are intended to indicate the presence of implemented features, numbers, steps, structural components, or a combination thereof, and they are not intended to exclude the possibility of the presence or addition of one or more other features, numbers, steps, structural components, or a combination thereof.

[0027] The terms “first”, “second”, “third”, etc. are used to explain various structural components, and they are used only to distinguish one structural component from other structural components.

[0028] As used herein, the term "polymer" refers to the polymerization state of water-soluble ethylenically unsaturated monomers, and may include polymers of all water content ranges or all particle size ranges. Among polymers, polymers that are not dried and have a water content of about 40% by weight or more may be referred to as hydrogel polymers, and ground and dried particles of such hydrogel polymers may be referred to as cross-linked polymers.

[0029] Furthermore, as used herein, "base resin" or "base resin powder" refers to particles or powders obtained by drying and grinding a polymer polymerized from an acrylic monomer before undergoing a surface modification or surface crosslinking step as described later.

[0030] In addition, the term "superabsorbent polymer" or "superabsorbent polymer powder" means a cross-linked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer containing an acid group at least a portion of which is neutralized, or a base resin powder composed of superabsorbent polymer particles obtained by grinding a cross-linked polymer, or a cross-linked polymer or base resin suitable for production including one made by subjecting it to additional processes such as surface cross-linking, fine powder reconstitution, drying, grinding and classification, etc.

[0031] Although the present invention can be modified in many ways and the present invention can have various forms, specific embodiments will be described and explained in detail below. However, it should be understood that this is not intended to limit the present invention to the specific disclosure, and the present invention includes all modifications, equivalents or replacements thereof without departing from the spirit and technical scope of the present invention.

[0032] Hereinafter, a preparation method of a super absorbent polymer and a super absorbent polymer according to specific embodiments of the present invention will be described in detail.

[0033] (Composition of superabsorbent polymer)

[0034] According to one embodiment of the present invention, a superabsorbent polymer composition is provided.

[0035] The composition of the superabsorbent polymer comprises: a superabsorbent polymer comprising a base resin and a surface crosslinked layer formed on the surface of the base resin, the base resin comprising a crosslinked polymer formed by crosslinking polymerization of an acrylic monomer having an acid group that is at least partially neutralized and an internal crosslinking agent, wherein the crosslinked polymer in the surface crosslinked layer is additionally crosslinked by a surface crosslinking agent; a aminoacetate (or salt) type chelating agent; and cysteine,

[0036] The aminoacetate (or salt) type chelating agent and cysteine ​​are each independently contained in the interior of the surface cross-linked layer or on the surface of the surface cross-linked layer.

[0037] Superabsorbent polymers are widely used in sanitary products such as diapers, sanitary pads, etc., and in this case, the after-use feeling may be reduced due to the odor of human and pet excrement. In addition, as the wearing time passes, bacteria grow faster due to the liquid absorbed in the product, thereby generating additional odor.

[0038] Previous deodorant materials contained in products to reduce odors should be used in excess to achieve a target degree of deodorizing ability, and thus absorption performance may be significantly deteriorated, and production costs may be increased.

[0039] Therefore, the inventors of the present disclosure have found that odors generated by various causes can be effectively controlled without deteriorating basic properties including absorption and water retention capacity of super absorbent polymers by using specific additives in combination, and have completed the present invention.

[0040] Specifically, according to the present disclosure, when the product is applied, both the primary odor generated by the odor-generating substances contained in body fluids, urine, etc., and the secondary odor generated by bacterial growth can be effectively controlled. In addition, by using the two additives in combination, excellent deodorizing ability and odor masking ability can be economically achieved in a relatively small amount, especially without reducing the absorption performance.

[0041] Glycine chelating agents are components that can effectively inhibit the growth of bacteria such as Escherichia coli caused by odor-generating substances. As the wearing time of the product passes, the bacterial growth is accelerated by the odor-generating substances remaining in the product, thereby generating additional odor, but the glycine chelating agents inhibit such bacterial growth to effectively reduce the generation of additional odor.

[0042] In particular, aminoacetate (or salt) type chelating agents are divalent cations that form salt cross-links between components of cell membranes, and they can effectively inhibit bacterial growth by destroying bacterial cell membranes.

[0043] Glycine (or salt) type chelating agents may include, for example, one or more selected from the group consisting of ethylenediaminetetraacetic acid (EDTA), L-glutamic acid diacetate (GLDA), methylglycine diacetic acid (MGDA), hydroxyethylethylenediaminetriacetic acid (HEDTA), ethanol diglycine (EDG), diethylenetriaminepentaacetic acid (DTPA) and their salts.

[0044] Based on 100 parts by weight of the base resin, the content of the aminoacetate (or salt) type chelating agent can be 0.01 to 3 parts by weight, and preferably, the content can be 0.025 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 2.5 parts by weight or less, 2.0 parts by weight or less, 1.5 parts by weight or less, or 0.01 to 2.5 parts by weight, 0.01 to 2.0 parts by weight, 0.025 to 3.0 parts by weight, 0.025 to 2.5 parts by weight, 0.05 to 2.5 parts by weight, 0.05 to 2.0 parts by weight, 0.1 to 2.5 parts by weight, or 0.1 to 2.0 parts by weight.

[0045] If used within the above content range, bacteria can be effectively inhibited without reducing the absorption performance, thereby significantly improving the deodorizing ability and odor masking ability of the absorbent polymer. The chelating agent can be mixed with the aqueous solution in the form of a salt and used, so the content range is based on the solid content. At the same time, if the content of the chelating agent is too small, the antibacterial properties of the target degree may not be achieved, and if the content of the chelating agent is too much, the unique characteristics of the superabsorbent polymer may be deteriorated.

[0046] Cysteine ​​can chemically react with odor-generating substances to reduce odor. Odor-generating substances generally have a small molecular weight, and they react with cysteine, thereby reducing or removing odor, and thus effectively suppress odor. In particular, cysteine ​​effectively reduces odors generated by aldehydes and ketones. Meanwhile, in the case of using similar amino acids such as methionine, deodorizing ability can be exhibited to a certain extent, but they have different main functional groups, so even if applied to SAP in the same amount, the absorption performance and deodorizing ability may be significantly deteriorated compared to cysteine.

[0047] Based on 100 parts by weight of the base resin, the content of cysteine ​​can be 0.01 parts by weight to 3 parts by weight, and preferably, the content is 0.025 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 2.5 parts by weight or less, 2.0 parts by weight or less, 1.5 parts by weight or less, or 0.01 parts by weight to 2.5 parts by weight, 0.01 parts by weight to 2.0 parts by weight, 0.025 parts by weight to 3.0 parts by weight, 0.025 parts by weight to 2.5 parts by weight, 0.05 parts by weight to 2.5 parts by weight, 0.05 parts by weight to 2.0 parts by weight, 0.1 parts by weight to 2.5 parts by weight, or 0.1 parts by weight to 2.0 parts by weight.

[0048] When used within the above content range, odor generation can be effectively suppressed without deteriorating absorption performance, thereby significantly improving the deodorizing ability and odor masking ability of the absorbent polymer. Cysteine ​​can be mixed with an aqueous solution in the form of a salt and used, so the content range is based on the solid content. However, if the content of cysteine ​​is too small, deodorizing performance may not be achieved, and if the content is too much, the unique characteristics of the super absorbent polymer may be deteriorated, and there may be process problems due to incomplete dissolution.

[0049] The base resin includes a cross-linked polymer formed by cross-linking polymerization of an acrylic monomer having an at least partially neutralized acid group and an internal cross-linking agent.

[0050] The acrylic monomer may be any monomer commonly used in the preparation of superabsorbent polymers. As a non-limiting example, the acrylic monomer may be a compound represented by the following Chemical Formula 1:

[0051] [Chemical formula 1]

[0052] R 1 -COOM 1

[0053] In Chemical Formula 1,

[0054] R 1 is a C2-5 alkyl group containing an unsaturated bond, M 1 It is a hydrogen atom, a monovalent or divalent metal, an ammonium group or an organic amine salt.

[0055] Preferably, the monomer may be one or more selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts thereof.

[0056] The acrylic monomer may have an acid group, and at least a portion of the acid group may be neutralized. Preferably, a monomer partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, ammonium hydroxide, etc. may be used.

[0057] Wherein, the neutralization degree of the monomer may be 40 mol% to 95 mol%, or 40 mol% to 80 mol%, or 45 mol% to 75 mol%. Although the range of the neutralization degree may vary depending on the final performance, if the neutralization degree is too high, the neutralized monomer may precipitate, and thus it may be difficult to smoothly polymerize, whereas if the neutralization degree is too low, the absorption power of the polymer may be significantly reduced, and may exhibit an elastic rubber-like property that is difficult to handle.

[0058] The "internal crosslinking agent" is used to distinguish it from the "surface crosslinking agent" used to crosslink the surface of the base resin, and it is used to crosslink the unsaturated bonds of the above-mentioned acryl-based monomer to perform polymerization. The crosslinking in this step does not distinguish between the surface or the inside, but is carried out through the surface crosslinking process of the base resin described later, and the surface of the super absorbent polymer particles finally prepared consists of a structure crosslinked by the surface crosslinking agent, and the inside consists of a structure crosslinked by the internal crosslinking agent.

[0059] As the internal crosslinking agent, any compound can be used as long as they can introduce crosslinking during the polymerization of the acrylic monomer. As a non-limiting example, as the internal crosslinking agent, a multifunctional crosslinking agent such as N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, 1,2-butanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerol tri(meth)acrylate, pentaerythritol tetraacrylate, triallylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerol or ethylene carbonate can be used alone or in combination, but is not limited thereto.

[0060] Such an internal crosslinking agent may be used at a concentration of 0.001 wt % to 1 wt %, or 0.01 wt % to 0.8 wt %, or 0.1 wt % to 0.7 wt % based on the monomer composition. If the concentration of the internal crosslinking agent is too low, the absorption rate of the polymer may decrease, and the gel strength may become weak. On the contrary, if the concentration of the internal crosslinking agent is too high, the absorption capacity of the superabsorbent polymer may decrease, and thus it may not be preferred as an absorbent.

[0061] In addition, the monomer composition may further contain additives such as a thickener, a plasticizer, an antiseptic stabilizer, an antioxidant, etc. as needed.

[0062] The super absorbent polymer includes a surface cross-linked layer formed on the surface of the base resin, wherein the cross-linked polymer is additionally cross-linked by a surface cross-linking agent.

[0063] Wherein, the aminoacetate (or salt) type chelating agent and cysteine ​​are each independently contained in the interior of the surface crosslinking layer or on the surface of the surface crosslinking layer. This means that the aminoacetate (or salt) type chelating agent and cysteine ​​are each independently added after the base resin is polymerized (= before the surface crosslinking step), during the surface crosslinking step or after the surface crosslinking step, which will be explained in detail in the preparation method of the superabsorbent polymer composition as described later.

[0064] The surface crosslinked layer is formed by additional crosslinking of the crosslinked polymer by a surface crosslinking agent, wherein the surface crosslinking agent is not particularly limited as long as it is generally used for surface crosslinking of superabsorbent polymers and is a compound capable of reacting with a functional group of the polymer.

[0065] Preferably, in order to improve the properties of the prepared superabsorbent polymer, as a surface crosslinking agent, one or more selected from the group consisting of polyol compounds, epoxy compounds, polyamine compounds, halogenated epoxy compounds, condensation products of halogenated epoxy compounds, oxazoline compounds, monooxazolidinone compounds, dioxazolidinone compounds or polyoxazolidinone compounds, cyclic urea compounds, polyvalent metal salts and alkylene carbonate compounds can be used.

[0066] Specifically, as examples of the polyol compound, one or more selected from the group consisting of monoethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol or polyethylene glycol, monopropylene glycol, 1,3-propylene glycol, dipropylene glycol, 2,3,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol and 1,2-cyclohexanedimethanol can be used.

[0067] Furthermore, as the epoxy compound, ethylene glycol diglycidyl ether, glycidol, etc. can be used, and as the polyamine compound, one or more selected from the group consisting of ethylenediamine, diethylenetriamine, triethylenetriamine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneamine, and polyamidepolyamine can be used.

[0068] Furthermore, as the halogenated epoxy compound, epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin can be used, and as the monooxazolidinone compound, dioxazolidinone compound, or polyoxazolidinone compound, for example, 2-oxazolidinone and the like can be used.

[0069] In addition, as the alkylene carbonate compound, ethylene carbonate and the like can be used. These compounds can be used alone or in combination. Meanwhile, in order to improve the efficiency of the surface crosslinking process, one or more C2-10 polyol compounds can be included in these surface crosslinking agents.

[0070] The content of the added surface crosslinking agent can be appropriately selected according to the type of the added surface crosslinking agent and the reaction conditions, but generally, based on 100 parts by weight of the polymer, its amount can be from about 0.001 parts by weight to about 5 parts by weight, preferably from about 0.01 parts by weight to about 3 parts by weight, and more preferably from about 0.05 parts by weight to about 2 parts by weight.

[0071] If the content of the surface crosslinking agent is too small, the surface crosslinking reaction may be difficult to occur, and if the content is greater than 5 parts by weight based on 100 parts by weight of the polymer, the absorption capacity and performance may be reduced due to excessive progress of the surface crosslinking reaction.

[0072] Meanwhile, the surface crosslinking agent can further comprise inorganic material.As such inorganic material, one or more in the group consisting of silicon dioxide, clay, aluminum oxide, silicon dioxide-alumina composite material, titanium dioxide, zinc oxide and aluminum sulfate can be used.Inorganic material can be used in the form of powder or liquid, particularly aluminum oxide powder, silicon dioxide-alumina powder, titanium dioxide powder or nano silicon dioxide solution.Based on the base resin of 100 weight parts, the usage amount of inorganic material can be from about 0.001 weight part to about 1 weight part.

[0073] In addition, the surface crosslinking agent may further include a thickener. If the surface of the base resin powder is additionally crosslinked in the presence of a thickener, performance degradation may be minimized even after grinding. Specifically, as a thickener, one or more selected from polysaccharides and hydroxyl-containing polymers may be used. As a polysaccharide, a gum-based thickener and a cellulose-based thickener may be used. As a specific example of a gum-based thickener, xanthan gum, gum arabic, gum karaya, gum tragacanth, gum ghatti, guar gum, locust bean gum and psyllium seed gum may be mentioned, and as a specific example of a cellulose-based thickener, hydroxypropyl methylcellulose, carboxymethyl cellulose, methylcellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methylcellulose and hydroxymethyl propyl cellulose, hydroxyethyl hydroxypropyl cellulose, ethyl hydroxyethyl cellulose and methyl hydroxypropyl cellulose may be mentioned. Meanwhile, as a specific example of a hydroxyl-containing polymer, polyethylene glycol and polyvinyl alcohol may be mentioned.

[0074] According to another embodiment of the present invention, the composition of the super absorbent polymer may further include one or more additives selected from the group consisting of metal iodide salts, organic acids and polyphenols, and through the additives, the deodorizing ability and the odor masking ability may be further improved.

[0075] The metal iodide salt may be, for example, in a form in which one or more selected from the group consisting of CuI, NaI, and KI and I2 are dissolved in water. The metal iodide salt may oxidize malodorous substances to impart deodorizing properties.

[0076] The organic acid may be, for example, one or more selected from the group consisting of citric acid, glutamic acid, ascorbic acid, benzoic acid, and isoascorbic acid.

[0077] The polyphenol may be, for example, one or more selected from the group consisting of tannins, anthocyanidins, flavonols, isoflavones, catechins, polyquercetin, and caffeic acid.

[0078] Based on 100 parts by weight of the base resin, preferably, the content of the additives may be each independently 0.025 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, 2.5 parts by weight or less, 2.0 parts by weight or less, 1.5 parts by weight or less, or 0.01 to 2.5 parts by weight, 0.01 to 2.0 parts by weight, 0.025 to 2.5 parts by weight, 0.05 to 2.5 parts by weight, 0.05 to 2.0 parts by weight, 0.1 to 2.5 parts by weight, or 0.1 to 2.0 parts by weight.

[0079] If used within the above range, they can achieve a synergistic effect with cysteine.

[0080] Meanwhile, if the content of the metal iodide salt is too much, it may reduce the unique properties of the super absorbent polymer and may be fed as a solution that increases residues during the process, thereby reducing the deodorizing ability instead. The metal iodide salt uses water as a solvent, is mixed with the super absorbent polymer in the state of an aqueous solution, and exists in the super absorbent polymer while being mixed and physically contained in the super absorbent polymer. The metal iodide salt may be a solution having a solid content concentration of 1% or less.

[0081] Meanwhile, the additives may be contained independently inside the surface crosslinked layer or on the surface of the surface crosslinked layer. This means that each additive is added during the polymerization of the base resin (= before the surface crosslinking step), in the surface crosslinking step, or after the surface crosslinking step, which will be explained in detail in the preparation method of the composition of the superabsorbent polymer described later.

[0082] (Method for preparing superabsorbent polymer composition)

[0083] According to one embodiment of the present invention, a method for preparing a superabsorbent polymer composition is provided.

[0084] The method for preparing a composition of a superabsorbent polymer comprises the following steps:

[0085] An acrylic monomer having an at least partially neutralized acid group is subjected to crosslinking polymerization in the presence of an internal crosslinking agent and a polymerization initiator to form a hydrogel polymer (step 1); a base resin comprising a crosslinked polymer obtained by drying and grinding the hydrogel polymer is prepared (step 2); a surface crosslinking composition is mixed with the base resin to prepare a mixture (step 3); and the mixture is heat-treated to prepare a superabsorbent polymer, wherein a surface crosslinked layer is formed on the surface of the base resin (step 4), wherein a aminoacetate (or salt) type chelating agent and cysteine ​​are each independently mixed in at least one of steps 2 to 4 and steps before and after these steps.

[0086] The preparation method of the superabsorbent polymer composition of the present invention can effectively control odors caused by various reasons by using a aminoacetate (or salt) chelating agent and cysteine ​​in combination, while not reducing the basic properties of the superabsorbent polymer, including absorption and water retention capacity. For the aminoacetate (or salt) chelating agent and cysteine, the above description is also applicable.

[0087] Meanwhile, the expression "mixed in step A" means additionally mixing with the target mixture while performing step A, and may also mean mixing in multiple times according to the target content ratio in the corresponding step. Meanwhile, the expression "mixed before and after step A" means additionally mixing before performing step A or after completing step A.

[0088] More specifically, aminoacetate (or salt) type chelating agent and cysteine ​​are mixed in at least one of steps 2 to 4 and steps before and after these steps, which means that they are mixed during the surface crosslinking step, before the surface crosslinking step, or after the surface crosslinking step is completed, and they can be mixed in one or more steps. The two additives are contained inside the surface crosslinking layer or on the surface of the surface crosslinking layer, thereby reacting with the odor-generating substance, having excellent deodorizing ability, inhibiting bacterial growth, and effectively inhibiting the generation of additional odor. At the same time, in the case of mixing the two additives in the polymerization step, it may be difficult to achieve the target effect.

[0089] More preferably, the aminoacetate (or salt) type chelating agent can be mixed in step 2, or mixed after step 4. More specifically, in the case where the chelating agent is included in the step (step 2) of preparing the base resin by the polymerized hydrogel polymer, it means that it is mixed with the base resin and added and mixed in the drying and grinding steps. In this case, the chelating agent can be included in the inside of the surface crosslinked layer formed in the surface crosslinking step. In addition, in the case where the chelating agent is mixed after the surface crosslinking step (step 4), it means that it is mixed with the superabsorbent polymer having the surface crosslinked layer. In this case, the chelating agent can be included on the surface of the surface crosslinked layer formed in the surface crosslinking step.

[0090] More preferably, cysteine ​​may be mixed after step 4. Specifically, in the case where cysteine ​​is mixed after the surface cross-linking step (step 4), it means that it is mixed with the super absorbent polymer having a surface cross-linked layer. In this case, the chelating agent may be contained on the surface of the surface cross-linked layer formed in the surface cross-linking step. In the case where cysteine ​​is contained after the surface cross-linking step (step 4), cysteine ​​is present on the surface of the super absorbent polymer, and therefore, the contact area with the odor may increase, which may be advantageous in terms of improving the deodorizing ability.

[0091] According to one embodiment of the present invention, in the method for preparing superabsorbent polymer, one or more additives selected from the group consisting of metal iodide salts, organic acids and polyphenols may be further included, and for these additives, the above descriptions are also applicable.

[0092] The additives may be mixed in at least one of steps 2 to 4 and steps before and after these steps, which means that they are mixed during the surface crosslinking step, before the surface crosslinking step, or after the surface crosslinking step is completed, and they may be mixed in one or more steps. Thus, the additives are contained inside the surface crosslinked layer or on the surface of the surface crosslinked layer, and the generation of odor can be more effectively suppressed.

[0093] More preferably, in the case where the additives are included after the surface crosslinking step (step 4), this means that they are mixed with the super absorbent polymer having a surface crosslinked layer. In this case, the additives are present on the surface of the surface crosslinked layer formed in the surface crosslinking step, and therefore, the contact area with the odor increases, which may be advantageous in terms of improving the deodorizing ability.

[0094] Hereinafter, the present invention will be described in detail according to the steps.

[0095] (Step 1)

[0096] Step 1 is a step of preparing a hydrogel polymer, and specifically, in this step, a monomer composition including an acrylic monomer having an at least partially neutralized acid group is cross-linked and polymerized to form a hydrogel polymer.

[0097] The acrylic monomer may be any monomer commonly used in preparing superabsorbent polymers. Specifically, for the acrylic monomer, the above description is also applicable.

[0098] Furthermore, in the monomer composition, a polymerization initiator generally used for preparing a super absorbent polymer may be included.

[0099] As the polymerization initiator, a thermal polymerization initiator or a photopolymerization initiator may be used according to the polymerization method. However, even when photopolymerization is performed, since a certain amount of heat is generated by UV irradiation or the like, and a certain degree of heat is generated according to the progress of the exothermic polymerization reaction, a thermal polymerization initiator may be additionally contained.

[0100] As the photopolymerization initiator, one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyalkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine and α-amino ketone can be used. Among them, as a specific example of acyl phosphine, commercially available Lucrin TPO, i.e. 2,4,6-trimethyl-benzoyl-trimethylphosphine oxide, can be used. More various photopolymerization initiators are described in Reinhold Schwalm's "UV Coatings: Basics, Recent Developments and New Applications" on page 115, which can be used as a reference.

[0101] And, as a thermal polymerization initiator, one or more selected from the group consisting of persulfate initiator, azo initiator, hydrogen peroxide and ascorbic acid can be used. Specific examples of persulfate initiators can include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), ammonium persulfate (NH4)2S2O8), etc., and specific examples of azo initiators can include 2,2-azobis (2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene) isobutylamidine dihydrochloride, 2-(carbamoyl azo) isobutyronitrile, 2,2-azobis [2-(2-imidazoline-2-yl) propane] dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. More various thermal polymerization initiators are described in Odian's "Principles of Polymerization (Wiley, 1981)" page 203, which can be used as a reference.

[0102] Such a polymerization initiator may be added at a concentration of 0.001 wt % to 1 wt % or 0.005 wt % to 0.1 wt % based on the monomer composition. If the concentration of the polymerization initiator is too low, the polymerization rate may be slowed down, and a large amount of residual monomers may be extracted in the final product. Also, if the concentration of the polymerization initiator is too high, the polymer chains constituting the superabsorbent polymer network may become shorter, and thus, the extractable content may increase, and the superabsorbent polymer pressure absorption rate may decrease, thereby deteriorating the performance of the polymer.

[0103] Meanwhile, the polymerization of the monomer composition is performed in the presence of an internal crosslinking agent to improve the properties of the polymer obtained by the polymerization of the acrylic monomer. As for the internal crosslinking agent, the aforementioned internal crosslinking agents may be applied in the same manner.

[0104] In addition, the cross-linking polymerization of the monomer composition may be performed in the presence of a foaming agent according to the necessity and degree of improving the absorption rate. Such a foaming agent may decompose and generate gas during the cross-linking polymerization reaction, thereby forming pores in the hydrogel polymer. Therefore, when such a foaming agent is additionally used, a more developed porous structure is formed in the superabsorbent polymer, and thus, the absorption rate of the superabsorbent polymer can be further improved.

[0105] As a non-limiting example, the foaming agent may include one or more compounds selected from the group consisting of sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, magnesium carbonate, azodicarbonamide (ADCA), dinitrosopentamethylenetetramine (DPT), p,p'-oxybis(benzenesulfonylhydrazide) (OBSH), p-toluenesulfonylhydrazide (TSH), sucrose stearate, sucrose palmitate, and sucrose laurate.

[0106] The content of the blowing agent in the monomer composition may be 1000 ppmw to 4000 ppmw, and more specifically, the content is 1000 ppmw or more, or 1100 ppmw or more, or 1200 ppmw or more, and 4000 ppmw or less, or 3500 ppmw or less, or 3000 ppmw or less.

[0107] Furthermore, the monomer composition may contain a thickener, a plasticizer, an antiseptic stabilizer, an antioxidant, and the like as necessary.

[0108] In addition, the monomer composition may be prepared in the form of a solution in which the above-mentioned raw materials, including the acrylic monomer, the polymerization initiator, the internal cross-linking agent, the foaming agent, etc., are dissolved in a solvent.

[0109] Among them, the solvent that can be used is not limited as long as it can dissolve the above raw materials. For example, as the solvent, water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide or a mixture thereof can be used.

[0110] The formation of the hydrogel polymer by polymerization of the monomer composition may be performed by a common polymerization method, and the process is not particularly limited.

[0111] As a non-limiting example, polymerization methods are roughly divided into thermal polymerization and photopolymerization according to the kind of energy source, and thermal polymerization can be performed in a reactor equipped with a stirring shaft (such as a kneader) and photopolymerization can be performed in a reactor equipped with a movable conveyor belt.

[0112] For example, the hydrogel polymer can be obtained by adding the above-mentioned monomer composition to a reactor (e.g., a kneader equipped with a stirring shaft) and supplying hot air or heating the reactor to perform thermal polymerization. The hydrogel polymer discharged to the reactor outlet can have a size of several centimeters to several millimeters depending on the shape of the stirring shaft equipped in the reactor. Specifically, the size of the obtained hydrogel polymer can vary according to the concentration and addition rate of the added monomer composition, and a hydrogel polymer with a particle size of 2 mm to 50 mm can usually be obtained.

[0113] For another example, in the case of photopolymerization of the monomer composition in a reactor equipped with a movable conveyor as described above, a hydrogel polymer in the form of a sheet can be obtained. The thickness of the sheet can vary depending on the concentration and addition rate of the added monomer composition, but it is generally preferred that the thickness of the sheet be controlled to be 0.5 cm to 10 cm so that the entire sheet can be polymerized uniformly and at the same time ensure production speed, etc.

[0114] The hydrogel polymer thus obtained may have a water content of 40% to 80% by weight. Wherein, "water content" refers to the content of water in the total weight of the hydrogel polymer, and refers to the value of subtracting the weight of the dry polymer from the weight of the hydrogel polymer. Specifically, it is defined as the value calculated by measuring the weight loss based on the evaporation of water in the polymer while raising the temperature of the polymer by infrared heating to dryness. Wherein, the temperature is increased from room temperature to about 180°C and then maintained at 180°C, and the total drying time can be set to 20 minutes, including a 5-minute heating step.

[0115] (Step 2)

[0116] Step 2 of the present disclosure is a step of drying and grinding the hydrogel polymer prepared in step 1 to form a base resin.

[0117] Specifically, in order to improve the drying efficiency of the hydrogel polymer, affect the morphology of the superabsorbent polymer, and thus affect various properties of the superabsorbent polymer, including the absorption speed, and in particular to improve the absorption speed of the superabsorbent polymer, the present disclosure may further include a coarse grinding step before drying the hydrogel polymer. Hereinafter, in order to distinguish it from the grinding after drying, for the sake of convenience, the grinding before drying is referred to as "coarse grinding" herein.

[0118] The grinding machine used for grinding is not limited, and specifically, may include any one selected from the group consisting of a vertical pulverizer, a turbine cutter, a turbine grinder, a rotary cutter, a cutter, a disc mill, a pulverizing crusher, a crusher, a shredder and a disc cutter, but is not limited thereto.

[0119] Among them, the rough grinding step may be performed so that the particle size of the hydrogel polymer may become about 2 mm to about 10 mm. Due to the high water content of the hydrogel polymer, grinding to a particle size of less than 2 mm is technically not easy, and it may cause aggregation between the ground particles. Meanwhile, if the grinding to a particle size greater than 10 mm, the effect of improving the efficiency of the subsequent drying step may not be significant.

[0120] Drying can be performed at a temperature of 120°C to 250°C, 140°C to 200°C, or 150°C to 190°C. The drying temperature can be defined as the temperature of the heat transfer medium supplied for drying or the temperature inside the drying reactor containing the heat transfer medium and the polymer during the drying process. If the drying temperature is too low and the drying time is prolonged, the process efficiency will be reduced. Therefore, in order to prevent this, the drying temperature is preferably above 120°C. In addition, if the drying temperature is higher than the required temperature, the surface of the hydrogel polymer may be over-dried, so the generation of fine powder may increase in the subsequent grinding step, and the properties of the final polymer may be deteriorated. Therefore, in order to prevent this, the drying temperature is preferably below 250°C.

[0121] The drying time in the drying step is not particularly limited, but can be controlled to be 20 minutes to 90 minutes at the above drying temperature in consideration of the processing efficiency and performance of the polymer.

[0122] Drying can be performed using common media, for example, drying can be performed by supplying hot air, infrared radiation, microwave radiation or UV radiation to the ground hydrogel polymer or the like.

[0123] In addition, preferably, drying is performed so that the water content of the dried polymer may be 0.1 wt % to 10 wt %. That is, in the case where the water content of the dried polymer is less than 0.1 wt %, the production cost may increase and the cross-linked polymer may deteriorate due to excessive drying. And, if the water content of the dried polymer is greater than 10 wt %, defects may occur in subsequent processes.

[0124] Subsequently, the dried hydrogel polymer may be ground. This is a step to optimize the surface area of ​​the base resin powder and the superabsorbent polymer. The grinding may be performed so that the particle size of the ground polymer may become 150 μm to 850 μm.

[0125] Among them, as the grinder, a common grinder such as a pin grinder, a hammer grinder, a spiral grinder, a roller grinder, a disc grinder, a tumble grinder, etc. can be used.

[0126] Furthermore, in order to control the properties of the finally produced super absorbent polymer, particles having a particle size ranging from 150 μm to 850 μm among the polymer particles obtained through the grinding step are subjected to a step of selectively classifying.

[0127] The base resin can be obtained by the classification step. The base resin may have a particle size of 150 μm to 850 μm, and may contain fine powder having a particle size of less than 150 μm at a content of 2 wt % or less, or 1 wt % or less.

[0128] Meanwhile, as described above, a glycine (or salt) type chelating agent may be included in the step of preparing a base resin from a polymerized hydrogel polymer (step 2), and in this case, aggregation of the base resin may be prevented, and thus performance degradation may be suppressed and the chelating agent may be more uniformly distributed. Meanwhile, the mixing method of the glycine (or salt) type chelating agent is not particularly limited, and may be mixed in a simple mixing manner or spray mixed in the state of an aqueous solution.

[0129] (Step 3 and Step 4)

[0130] Step 3 of the present disclosure is a step of mixing the base resin prepared in step 2 with the surface crosslinking composition, and step 4 is a step of heat-treating the mixture to prepare a superabsorbent polymer having a surface crosslinking layer formed on the surface of the base resin.

[0131] The surface crosslinking composition used in step 3 comprises a surface crosslinking agent, and the surface crosslinking agent is not particularly limited as long as it is commonly used for surface crosslinking of super absorbent polymers and is a compound capable of reacting with functional groups of polymers.

[0132] Preferably, in order to improve the properties of the prepared superabsorbent polymer, as a surface crosslinking agent, one or more selected from the group consisting of polyol compounds, epoxy compounds, polyamine compounds, halogenated epoxy compounds, condensation products of halogenated epoxy compounds, oxazoline compounds, monooxazolidinone compounds, dioxazolidinone compounds or polyoxazolidinone compounds, cyclic urea compounds, polyvalent metal salts and alkylene carbonate compounds can be used.

[0133] Specifically, as examples of the polyol compound, one or more selected from the group consisting of monoethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol or polyethylene glycol, monopropylene glycol, 1,3-propylene glycol, dipropylene glycol, 2,3,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerol, polyglycerol, 2-butene-1,4-diol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol and 1,2-cyclohexanedimethanol can be used.

[0134] Furthermore, as the epoxy compound, ethylene glycol diglycidyl ether, glycidol, etc. can be used, and as the polyamine compound, one or more selected from the group consisting of ethylenediamine, diethylenetriamine, triethylenetriamine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneamine, and polyamidepolyamine can be used.

[0135] Furthermore, as the halogenated epoxy compound, epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin can be used, and as the monooxazolidinone compound, dioxazolidinone compound, or polyoxazolidinone compound, for example, 2-oxazolidinone and the like can be used.

[0136] In addition, as the alkylene carbonate compound, ethylene carbonate and the like can be used. These compounds can be used alone or in combination. Meanwhile, in order to improve the efficiency of the surface crosslinking process, one or more C2-10 polyol compounds can be included in these surface crosslinking agents.

[0137] The content of the added surface crosslinking agent can be appropriately selected according to the type of the added surface crosslinking agent and the reaction conditions, but generally, based on 100 parts by weight of the polymer, its amount can be from about 0.001 parts by weight to about 5 parts by weight, preferably from about 0.01 parts by weight to about 3 parts by weight, and more preferably from about 0.05 parts by weight to about 2 parts by weight.

[0138] If the content of the surface crosslinking agent is too small, the surface crosslinking reaction may be difficult to occur, and if the content is greater than 5 parts by weight based on 100 parts by weight of the polymer, the absorption capacity and performance may be reduced due to excessive progress of the surface crosslinking reaction.

[0139] Simultaneously, can carry out the step of forming surface crosslinking layer when the surface crosslinking agent further comprises inorganic material.As such inorganic material, can use one or more in the group being selected from by silicon dioxide, clay, aluminum oxide, silicon dioxide-alumina composite material, titanium dioxide, zinc oxide and aluminum sulfate.Inorganic material can be used in the form of powder or liquid, particularly aluminum oxide powder, silicon dioxide-alumina powder, titanium dioxide powder or nano silicon dioxide solution.Based on the base resin of 100 weight parts, the usage amount of inorganic material can be about 0.001 weight part to about 1 weight part.

[0140] In addition, the surface cross-linked composition may further include a thickener. If the surface of the base resin powder is additionally cross-linked in the presence of a thickener, performance degradation may be minimized even after grinding. Specifically, as a thickener, one or more selected from polysaccharides and hydroxyl-containing polymers may be used. As a polysaccharide, a gum-based thickener and a cellulose-based thickener may be used. As a specific example of a gum-based thickener, xanthan gum, gum arabic, gum karaya, gum tragacanth, gum ghatti, guar gum, locust bean gum and psyllium seed gum may be mentioned, and as a specific example of a cellulose-based thickener, hydroxypropyl methylcellulose, carboxymethyl cellulose, methylcellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methylcellulose and hydroxymethyl propyl cellulose, hydroxyethyl hydroxypropyl cellulose, ethyl hydroxyethyl cellulose and methyl hydroxypropyl cellulose may be mentioned. Meanwhile, as a specific example of a hydroxyl-containing polymer, polyethylene glycol and polyvinyl alcohol may be mentioned.

[0141] Meanwhile, the mixing method of the base resin and the surface cross-linking composition may be appropriately selected without specific limitation as long as they can be uniformly mixed.

[0142] For example, a method of placing the surface crosslinking composition and the base resin in a reactor and mixing them, a method of spraying the surface crosslinking composition onto the surface of the base resin, a method of continuously feeding the base resin and the surface crosslinking composition into a continuously operated mixer and mixing them, etc. can be used.

[0143] Among them, the surface cross-linking composition can be a solution. When the solid content in the solution is more than 1 weight %, more than 3 weight %, more than 5 weight %, more than 10 weight %, and less than 50 weight %, less than 30 weight %, or less than 20 weight %, it can be appropriately and evenly dispersed in the base resin and the base resin can be prevented from agglomerating.

[0144] Next, step 4 is a step of heat-treating the mixture to prepare a super absorbent polymer in which a surface cross-linked layer is formed on the surface of the base resin, and specifically, the base resin and the surface cross-linked composition are heat-treated to form an interpenetrating polymer network on the surface of the cross-linked polymer contained in the base resin, thereby further improving the performance of the super absorbent polymer. Through this surface modification, a surface cross-linked layer is formed on the surface of the ground base resin particles.

[0145] The formation of the surface crosslinked layer can be performed by a common method of increasing the crosslinking density of the polymer particle surface, and for example, it can be performed by mixing the ground polymer with a surface crosslinking solution containing a surface crosslinking agent and heat-treating the mixture to cause it to undergo a crosslinking reaction.

[0146] Step 4 may be performed at a temperature of about 80° C. to about 250° C. More specifically, the surface crosslinking process may be performed at a temperature of about 100° C. to about 220° C., or about 110° C. to about 200° C., or about 120° C. to about 190° C. for about 10 minutes to about 2 hours, or about 20 minutes to about 60 minutes. If the crosslinking reaction temperature is less than 160° C. or the reaction time is too short, the surface crosslinking reaction may not sufficiently occur, and thus the degree of penetration may be reduced, and if the crosslinking reaction temperature is greater than 200° C. or the reaction time is too long, the water retention capacity may be reduced.

[0147] There is no specific restriction on the heating mode of the surface cross-linking reaction. A heat transfer medium can be supplied, or a heat source can be directly supplied for heating. Among them, as the type of heat transfer medium that can be used, a heating fluid such as steam, hot air, hot oil can be used, but the present invention is not limited thereto, and the temperature of the supplied heat transfer medium can be appropriately selected by considering the mode of the heat transfer medium, the heating mode and the target temperature. At the same time, as the heat source directly supplied, electric heating and gas heating can be mentioned, but the present disclosure is not limited thereto.

[0148] Meanwhile, as described above, a aminoacetate (or salt) type chelating agent may be mixed after the step of heat-treating the mixture to prepare a superabsorbent polymer having a crosslinked layer formed on the surface of the base resin (step 4), which is advantageous in that the possibility of generating residues when treated with cysteine, etc. after surface crosslinking can be further reduced. Meanwhile, there is no particular limitation on the mixing method of the aminoacetate (or salt) type chelating agent, and the mixing may be performed by simple mixing or spray mixing in the state of an aqueous solution.

[0149] In addition, as described above, cysteine ​​may be mixed after the step of heat-treating the mixture to prepare a super absorbent polymer having a cross-linked layer formed on the surface of the base resin (step 4), which is advantageous because the cross-linked layer exists on the surface of the super absorbent polymer to increase the contact area with the odor, thereby improving the deodorizing ability. Meanwhile, there is no particular limitation on the mixing method of cysteine, and the mixing may be performed by spraying in an aqueous solution state or dry mixing.

[0150] Further, after the step of heat-treating the mixture, one or more additives selected from the group consisting of metal iodide salts, organic acids and polyphenols may be mixed to prepare a super absorbent polymer having a cross-linked layer formed on the surface of the base resin (step 4), which is advantageous because the cross-linked layer exists on the surface of the super absorbent polymer to increase the contact area with the odor, thereby improving the deodorizing ability. Meanwhile, there is no specific limitation on the mixing method of the additives, and the mixing may be performed by spraying in an aqueous solution state or dry mixing.

[0151] According to one embodiment of the present invention, after the step of preparing a super absorbent polymer having a cross-linked layer formed on the surface of a base resin (step 4), a step of mixing aminoacetate (or salt) type chelating agent, cysteine, metal iodide salt, organic acid and polyphenol in the form of an aqueous solution (a step of adding after hydration) may be included, and in this case, a drying step may be additionally performed. For the drying process, the above description is also applicable.

[0152] Hereinafter, preferred examples are given to help understand the present invention. However, the following examples are given only as illustrations of the present invention and are not intended to limit the present invention.

[0153] Examples and Comparative Examples: Preparation of Superabsorbent Polymers

[0154] Example 1

[0155] (Step 1) 100 g of acrylic acid, 0.37 g of N,N'-methylenebisacrylamide as a crosslinking agent, 0.15 g of sodium persulfate (SPS) as a thermal initiator, 0.008 g of benzoin ether as a UV initiator, 40 g of caustic soda (NaOH) and 127 g of water were mixed to prepare an aqueous monomer composition having a monomer concentration of 45.8 wt%. The aqueous monomer composition was introduced into a feed section of a polymerization reactor equipped with a continuously moving conveyor belt, and then, while maintaining the polymerization atmosphere temperature at 80°C, was irradiated with a UV irradiation device (dosage: 10 mW / cm 2 ) was irradiated with UV and subjected to UV polymerization for 2 minutes to prepare a hydrogel polymer.

[0156] (Step 2) The hydrogel polymer was transferred to a meat chopper and cut into 2 mm to 10 mm. The water content of the cut hydrogel polymer was 47% by weight. Subsequently, the hydrogel polymer was dried in a hot air dryer at 170° C. for 30 minutes, and the dried hydrogel polymer was ground with a pin grinder. Subsequently, the polymer having a particle size (average particle size) of 150 μm to 850 μm was classified with a sieve to prepare a base resin.

[0157] (Step 3) A surface crosslinking solution (2.5 parts by weight of water, 0.1 parts by weight of ethylene glycol diglycidyl ether (EX-810), 0.1 parts by weight of aluminum sulfate 18 hydrate (Al-S), and 0.1 parts by weight of silica (Aerosil A200)) was uniformly mixed into 100 parts by weight of the base resin prepared above.

[0158] (Step 4) Next, a surface crosslinking reaction was carried out at 140° C. for 30 minutes. After the surface treatment was completed, a super absorbent polymer having an average particle size of 150 μm to 850 μm was obtained by classification with a sieve. In the super absorbent polymer thus obtained, the content of the polymer having an average particle size of less than 150 μm was less than 2%.

[0159] In step 2, EDTA is dissolved in an aqueous solution as a aminoacetate (or salt) type chelating agent to mix EDTA, and sprayed onto the base resin to a concentration of 0.5 parts by weight based on 100 parts by weight of the base resin.

[0160] Further, after the surface crosslinking in step 4, L-cysteine ​​is mixed by dissolving L-cysteine ​​in an aqueous solution and sprayed on the super absorbent polymer to a concentration of 0.2 parts by weight based on 100 parts by weight of the base resin. Thereafter, a drying step is performed to prepare a composition of the super absorbent polymer.

[0161] Examples 2 to 17, and Comparative Examples 1 to 3

[0162] A superabsorbent polymer was prepared by the same method as in Example 1, except that the components, contents and addition time of the additives in Example 1 were changed as shown in Table 1.

[0163] Meanwhile, in Examples 9 to 11, additional additives were sprayed on the surface-crosslinked superabsorbent polymer in the form of an aqueous solution (metal iodide salt solution (1% concentration, CuI), tannin solution, citric acid solution), and an additional drying step was performed.

[0164] [Table 1]

[0165]

[0166] Experimental example

[0167] For the superabsorbent polymer compositions prepared in Examples and Comparative Examples, properties thereof were measured as follows.

[0168] (1) Evaluation of absorption performance

[0169] 1) Centrifugal Retention Capacity (CRC)

[0170] The centrifuge retention capacity of each superabsorbent polymer composition of Examples and Comparative Examples was measured by the absorbency under no load according to EDANA WSP 241.3 of the European Disposables and Nonwovens Association (EDANA) standard.

[0171] Specifically, a polymer graded with a sieve of #30-50 was obtained from each composition of superabsorbent polymer obtained by Examples and Comparative Examples. Such a polymer W0 (g, about 0.2 g) was uniformly placed in an envelope made of non-woven fabric, and the envelope was sealed and then immersed in a 0.9 wt % saline solution. After 30 minutes, the envelope was drained at 250G for 3 minutes using a centrifuge, and the weight W2 (g) of the envelope was measured. In addition, the same operation was performed using an empty envelope containing no polymer, and then the weight W1 (g) at that time was measured.

[0172] Using the weight thus obtained, CRC (g / g) was confirmed by the following Mathematical Formula 1.

[0173] [Mathematical formula 1]

[0174] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1

[0175] 2) AUP: Absorption Percentage Under Pressure (AUP)

[0176] For each superabsorbent polymer composition of Examples and Comparative Examples, the pressure absorption rate at 0.7 psi was measured according to EDANA method WSP 242.3.

[0177] First, when measuring the pressure absorption rate, the graded polymers used for measuring CRC are used.

[0178] Specifically, a 400-mesh stainless steel wire mesh was installed at the bottom of a plastic cylinder with an inner diameter of 25 mm. And, under the conditions of room temperature and 50% humidity, W0 (g) of superabsorbent polymer was evenly dispersed on the mesh, and a piston capable of evenly applying a load of 0.7 psi was placed thereon, wherein a piston with an outer diameter slightly smaller than 25 mm was used so that there was no gap with the inner wall of the cylinder and the up and down movement was not hindered. At this time, the weight of the device was measured W3 (g).

[0179] In a petri dish with a diameter of 150 mm, a glass filter with a diameter of 90 mm and a thickness of 5 mm is placed, and a 0.9 wt% saline solution is poured to the same height as the upper side of the glass filter. And, a filter paper with a diameter of 90 mm is placed on it. Then, the above-mentioned measuring device is placed on the filter paper, and the solution is absorbed under pressure for 1 hour. After 1 hour, the measuring device is lifted and the weight W4 (g) is measured. Using the measured weight, the pressure absorption rate (g / g) is calculated according to the following mathematical formula 2.

[0180] [Mathematical formula 2]

[0181] AUP(g / g)=[W4(g)-W3(g)] / W0(g)

[0182] (2) Evaluation of antibacterial rate

[0183] The antibacterial rate of each superabsorbent polymer composition of Examples and Comparative Examples was evaluated as follows.

[0184] Specifically, commercial Escherichia coli (Escherichia Coli ATCC25922) was cultured in LB broth for 24 hours, and then the cultured bacteria were diluted and injected into 2 g samples of each superabsorbent polymer composition together with artificial urine, cultured at 37°C for 24 hours, and then the bacteria were extracted and the number of bacteria was measured (the average value of 2 samples).

[0185] Bacterial inhibition rate (%) = (1-((bacterial quantity of sample) / (bacterial quantity of reference sample (sample without deodorizing ability))))) X 100 (%)

[0186] The experimental results of the antibacterial rate are shown in Table 2. The numerical values ​​in Table 2 indicate the deodorization efficiency compared with Comparative Example 1, and the higher the numerical value, the higher the deodorization efficiency.

[0187] (3) Deodorization ability (deodorization rate)

[0188] The deodorizing ability was measured by the adsorption tube measurement method. As malodorous substances, ketone (diacetyl), sulfur compound (dimethyl trisulfide) and aldehyde (3-methylbutyraldehyde) were selected and the deodorizing ability was tested.

[0189] -Adsorption tube measurement method: 1g of super absorbent polymer is placed in a 500mL glass bottle, and then 25mL of malodorous substances are introduced. Then, aging is performed in a constant temperature chamber for 3 hours, and then capture is performed for 20 minutes. Among them, the constant temperature chamber temperature is 35°C and the N2 flow rate is 230mL / min. The discharged odor is then adsorbed to the connected adsorption tube, and the same sample is repeated twice for capture. The capture results are confirmed by GC analysis.

[0190] - Deodorization rate (%) = [odor amount of reference sample (sample without deodorization ability) measured by GC - odor amount of sample measured by GC] / odor amount of reference sample (sample without deodorization ability) measured by GC × 100 (%)

[0191] The results of the deodorizing ability test are shown in Table 2. The numerical values ​​in Table 2 indicate the deodorizing efficiency compared with Comparative Example 1, and the higher the numerical value, the higher the deodorizing efficiency.

[0192] [Table 2]

[0193]

[0194] According to the results in Table 2, it can be confirmed that by combining the aminoacetate (or salt) chelating agent and cysteine, the composition of the superabsorbent polymer of the embodiment of the present disclosure exhibits excellent absorption performance, while having excellent deodorizing ability and odor masking ability, and can effectively inhibit bacterial growth during product wearing.

[0195] It can be confirmed that in the case of the comparative example using only a part of the two additives, it is difficult to achieve both the antibacterial rate and the deodorizing ability. In particular, when a metal salt of ricinoleic acid is used in place of an aminoacetic acid root (or salt) type chelating agent in combination with cysteine, although the deodorizing ability is similar to that of the embodiment, the bacterial growth inhibition rate is significantly low.

Claims

1. A composition of a superabsorbent polymer, comprising: A superabsorbent polymer comprising a base resin and a surface crosslinked layer formed on a surface of the base resin, the base resin comprising a crosslinked polymer formed by crosslinking polymerization of an acrylic monomer having an at least partially neutralized acid group and an internal crosslinking agent, wherein the crosslinked polymer in the surface crosslinked layer is additionally crosslinked by the surface crosslinking agent; Glycine chelating agents; and Cysteine, The aminoacetate (or salt) type chelating agent and the cysteine ​​are each independently contained in the interior of the surface cross-linked layer or on the surface of the surface cross-linked layer.

2. The superabsorbent polymer composition according to claim 1, wherein The aminoacetate (or salt) chelating agent includes one or more selected from the group consisting of ethylenediaminetetraacetic acid (EDTA), L-glutamic acid diacetate (GLDA), methylglycine diacetic acid (MGDA), hydroxyethylethylenediaminetriacetic acid (HEDTA), ethanol diglycine (EDG), diethylenetriaminepentaacetic acid (DTPA) and their salts.

3. The superabsorbent polymer composition according to claim 1, wherein The aminoacetate (or salt) based chelating agent is included in an amount of 0.01 to 3 parts by weight based on 100 parts by weight of the base resin.

4. The superabsorbent polymer composition according to claim 1, wherein The cysteine ​​may be included in an amount of 0.01 to 3 parts by weight based on 100 parts by weight of the base resin.

5. The superabsorbent polymer composition according to claim 1, wherein It further comprises one or more additives selected from the group consisting of metal iodide salts, organic acids and polyphenols.

6. A method for preparing a composition of a superabsorbent polymer, comprising the following steps: Step 1: In the presence of an internal crosslinking agent and a polymerization initiator, crosslinking and polymerizing an acrylic monomer having an acid group that is at least partially neutralized to form a hydrogel polymer; Step 2: preparing a base resin comprising a cross-linked polymer obtained by drying and grinding the hydrogel polymer; Step 3: mixing a surface cross-linking composition with the base resin to prepare a mixture; and Step 4: heat-treating the mixture to prepare the super absorbent polymer, wherein a surface cross-linked layer is formed on the surface of the base resin, Wherein, in at least one of steps 2 to 4 and the steps before and after these steps, the aminoacetate (or salt) type chelating agent and cysteine ​​are mixed independently.

7. The method for preparing a superabsorbent polymer composition according to claim 6, wherein: The aminoacetate (or salt) chelating agent is mixed in step 2 or after step 4.

8. The method for preparing a superabsorbent polymer composition according to claim 6, wherein: The cysteine ​​is mixed after step 4.

9. The method for preparing a superabsorbent polymer composition according to claim 6, wherein: The preparation method further comprises the step of mixing at least one additive selected from the group consisting of metal iodide salts, organic acids and polyphenols.

10. The method for preparing a superabsorbent polymer composition according to claim 9, wherein: The additives are each independently mixed in at least one of steps 2 to 4 and steps before and after these steps.

11. The method for preparing a superabsorbent polymer composition according to claim 9, wherein: The additives are mixed independently after step 4.