Asymmetric laminated sodium-based composite solid electrolyte, preparation method thereof and battery
By using an asymmetric stacked sodium-based composite solid electrolyte in a sodium-ion battery, and utilizing the conductive agent and polymer matrix of the second composite solid electrolyte layer to form ion/electron hybrid conductive characteristics, the electrolyte leakage and leakage of traditional sodium-ion batteries are solved. The problem of poor thermal stability improves the stability and cycle life of the battery.
Patent Information
- Application Number
- CN202380015221.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-10-08
AI Technical Summary
Traditional sodium-ion batteries have problems such as electrolyte leakage, flammability, and poor thermal stability, resulting in low battery stability and reversible capacity loss, which hinders the development and large-scale application of sodium-ion batteries.
Using an asymmetric laminated sodium-based composite solid electrolyte, a second composite solid electrolyte layer containing a polymer matrix, sodium salt and conductive agent is provided on the negative electrode side, combined with the first composite solid electrolyte layer, to form ion/electron hybrid conductive properties , improve the stability of the negative electrode side interface and the sodium ion transmission efficiency.
It achieves high interface stability and long-cycle charge/discharge performance on the negative side of the sodium-ion battery, improves the cycle life and electrochemical performance of the battery, and solves the safety and stability problems of traditional sodium-ion batteries.
Smart Images

Figure CN118749145A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and more specifically, to an asymmetric laminated sodium-based composite solid electrolyte and a preparation method thereof and a battery. Background Art
[0002] Sodium-ion batteries (SIBs) have the advantages of high energy efficiency and abundant sodium resources, making them very promising for use in electric vehicles, fixed energy supply systems and mobile power sources. They are considered to be the best candidate to replace lithium-ion batteries in the future large-scale energy storage field. However, traditional sodium-ion batteries based on organic liquid electrolytes have problems such as electrolyte leakage, flammability and poor thermal stability. In addition, the morphology and orientation of sodium dendrite growth are uncontrollable, which will reduce battery stability or form "dead sodium" leading to reversible capacity loss of SIBs, hindering the development and large-scale application of SIBs. Summary of the invention
[0003] In view of the deficiencies in the prior art, one of the purposes of the present invention is to solve one or more problems in the prior art. For example, one of the purposes of the present invention is to provide an asymmetric laminated sodium-based composite solid electrolyte that can improve the interface stability and long-cycle charge / discharge performance of a sodium ion battery negative electrode side.
[0004] One aspect of the present invention provides an asymmetric laminated sodium-based composite solid electrolyte, which may include a first composite solid electrolyte layer adjacent to a positive electrode, and a second composite solid electrolyte layer arranged between the first composite solid electrolyte layer and the negative electrode, wherein the first composite solid electrolyte layer comprises a polymer matrix and a sodium salt; the second composite solid electrolyte layer comprises a polymer matrix, a sodium salt and a conductive agent, wherein the conductive agent accounts for 1% to 10% of the mass of the second composite solid electrolyte layer.
[0005] Furthermore, the first composite solid electrolyte layer also contains inorganic fillers, wherein the mass percentage of each component in the first composite solid electrolyte layer can be: 15-95% polymer matrix, 0.5%-70% inorganic filler, and the molar ratio of sodium salt to polymer monomer can be (0-1):20.
[0006] Furthermore, the second composite solid electrolyte layer also contains inorganic fillers, wherein the mass percentage of each component in the second composite solid electrolyte layer is: 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler, and the molar ratio of the sodium salt to the polymer monomer is (0 to 1):20.
[0007] Furthermore, the first composite solid electrolyte layer also includes a plasticizer, and the mass percentage of the plasticizer in the first composite solid electrolyte layer is 0.5% to 20%; the mass percentage of the plasticizer in the second composite solid electrolyte layer is 0.5% to 20%.
[0008] Furthermore, the mass ratio of the first composite solid electrolyte layer to the second composite solid electrolyte layer is (1-8):1.
[0009] Further, the polymer matrix is selected from at least one of polyethylene oxide, polyacrylonitrile, poly(methyl methacrylate), poly(vinyl alcohol), polyvinyl pyrrolidone, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene), polypropylene carbonate and polyvinyl carbonate;
[0010] Inorganic fillers are selected from Si, Al2O3, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3) and NaMM′P3O 12 At least one of, wherein M and M' are Si 2+ Mg 2+ , Cu 2+ 、Co 2+ 、Zn 2+ , Mn 2+ , Fe 2+ 、Al 3+ Cr 3+ Sc 3+ , Y 3+ ,La 3+ 、Ti 4+ 、Zr 4+ ,Ge 4+ Sn 4+ , Nb 4+ 、V 5+ , Nb 5+ and Ta 5+ Any of the following:
[0011] The sodium salt is selected from at least one of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI and sodium bis(oxalatoborate);
[0012] The plasticizer is selected from at least one of succinonitrile, polystyrene, ethylene carbonate, propylene carbonate, polyethylene glycol, polyethylene glycol dimethyl ether, tetraethylene glycol, triethylene glycol dimethyl ether, diethyl phthalate, dioctyl phthalate, cyclic phosphate, dibutyl phthalate and dimethyl phthalate;
[0013] The conductive agent is selected from at least one of graphite, graphene, carbon nanotubes, acetylene black and Ketjen black.
[0014] Another aspect of the present invention provides a method for preparing the asymmetric laminated sodium-based composite solid electrolyte as described above, which may include the following steps: mixing a polymer matrix, an inorganic filler, a sodium salt, a plasticizer and an organic solvent to obtain a first composite solid electrolyte slurry; applying the first composite solid electrolyte slurry to a mold, and drying it with air to obtain a first composite solid electrolyte layer; mixing a polymer matrix, an inorganic filler, a sodium salt, a plasticizer, a conductive agent and an organic solvent to obtain a second composite solid electrolyte slurry; coating the second composite solid electrolyte slurry on the first composite solid electrolyte layer, and drying it with air and vacuum drying to obtain an asymmetric laminated sodium-based composite solid electrolyte.
[0015] Further, the organic solvent in the first composite solid electrolyte slurry and the second composite solid electrolyte slurry is one or a combination of acetone, N,N-dimethylformyl and nitrogen methyl pyrrolidone;
[0016] Alternatively, the organic solvent is a mixture of acetone and N,N-dimethylformyl in a mass ratio of (1-25):1;
[0017] Alternatively, the organic solvent is a mixed solution of acetone and nitrogen methyl pyrrolidone in a mass ratio of (1-25):1.
[0018] Another aspect of the present invention provides a sodium ion battery, which may include a positive electrode, a negative electrode, and an asymmetric layered sodium-based composite solid electrolyte as described above located between the positive electrode and the negative electrode, or an asymmetric layered sodium-based composite solid electrolyte prepared by the preparation method as described above.
[0019] Compared with the prior art, the present invention has at least one of the following beneficial effects:
[0020] (1) The second composite solid electrolyte layer of the asymmetric stacked sodium-based composite solid electrolyte of the present invention is adjacent to the negative electrode of the battery, so that the negative electrode side of the battery has ion / electron mixed conductive properties, which can improve the interface contact between the negative electrode and the solid electrolyte and release the local accumulated charges on the negative electrode side interface and the rapid transmission of sodium ions and the uniform deposition of sodium ions, thereby achieving high interface stability and high long-cycle charge / discharge performance on the negative electrode side of the sodium ion battery.
[0021] (2) The asymmetric layered sodium-based composite solid electrolyte of the present invention has stable cycle performance and high electron transfer rate, and the battery formed has good initial electrochemical performance.
[0022] (3) The asymmetric layered sodium-based composite solid electrolyte of the present invention can improve the cycle life and electrochemical performance of sodium ion batteries after being assembled into batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The above and other objects and features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0024] Figure 1 A plan SEM image of the first composite solid electrolyte layer prepared in Example 1 of the present invention is shown.
[0025] Figure 2 A plan SEM image of the second composite solid electrolyte layer prepared in Example 1 of the present invention is shown.
[0026] Figure 3 The cross-sectional SEM image of the composite solid electrolyte prepared in Example 1 of the present invention is shown.
[0027] Figure 4 The structure diagram of the composite solid electrolyte sodium ion battery prepared in Example 1 of the present invention is shown.
[0028] Figure 5 The Na||Na symmetric battery charge and discharge cycle curve corresponding to the composite solid electrolyte prepared in Example 1 of the present invention is shown.
[0029] Figure 6 The Na||Na symmetric battery charge and discharge cycle curve corresponding to the composite solid electrolyte prepared in Comparative Example 1 of the present invention is shown.
[0030] Figure 7 The Na||Na3V2(PO4)3 battery charge and discharge curves corresponding to the composite solid electrolytes prepared in Example 1 of the present invention and Comparative Example 1 are shown.
[0031] Figure 8 The Na||Na3V2(PO4)3 battery charge and discharge curves corresponding to the composite solid electrolytes prepared in Examples 2 and 3 of the present invention are shown.
[0032] Fig. 9 The Na||Na3V2(PO4)3 battery rate performance curves corresponding to the composite solid electrolytes prepared in Example 2 of the present invention and Comparative Example 2 are shown. DETAILED DESCRIPTION
[0033] Hereinafter, an asymmetric laminated sodium-based composite solid electrolyte, a preparation method thereof, and a battery according to the present invention will be described in detail with reference to the accompanying drawings and exemplary embodiments.
[0034] Specifically, for batteries, solid-state sodium-ion batteries assembled with solid electrolytes instead of electrolytes can fundamentally solve safety problems such as leakage, volatilization, gas production and flammability of traditional sodium-ion battery electrolytes. In addition, solid-state sodium-ion batteries have the advantages of high energy density and being green and pollution-free, providing strong conditions for realizing high-energy density batteries, miniaturized batteries and developing green energy.
[0035] The present invention provides an asymmetric laminated sodium-based composite solid electrolyte. The continuous and tight ion / electron mixed conductive layer on the negative electrode side (second composite solid electrolyte layer) of the composite solid electrolyte is conducive to the uniform and rapid diffusion and deposition of electrons and sodium ions at the interface, inhibits the growth of sodium dendrites, achieves high negative electrode / solid electrolyte interface stability, and can improve the cycle life and electrochemical performance of sodium ion batteries.
[0036] One aspect of the present invention provides an asymmetric laminated sodium-based composite solid electrolyte. In some embodiments, Figure 3 As shown, the asymmetric laminated sodium-based composite solid electrolyte may include a first composite solid electrolyte layer 31 and a second composite solid electrolyte layer 32 connected to the first composite solid electrolyte layer. The first composite solid electrolyte layer is connected to the positive electrode of the battery and is located on the positive electrode side of the battery; the second solid electrolyte layer is connected to the negative electrode of the battery and is located on the negative electrode side of the battery. Since the first composite solid electrolyte layer and the second composite solid electrolyte layer have different components, the composite solid electrolyte is asymmetric.
[0037] The first composite solid electrolyte layer may include a polymer matrix, an inorganic filler, a sodium salt and a plasticizer (to increase the plasticity and film-forming properties of the polymer).
[0038] The second composite solid electrolyte layer may include a polymer matrix, an inorganic filler, a sodium salt, a plasticizer, and a conductive agent, wherein the conductive agent accounts for 1% to 10% of the mass of the second composite solid electrolyte layer. At present, the existing conventional solid electrolyte and the negative electrode contact interface are microscopically point contact, which will lead to uneven sodium ion transmission channels and charge distribution between the contact point and the non-contact point. The solid electrolyte of the present invention has an ion / electron mixed conductive characteristic interface with the negative electrode, which can effectively disperse the charges accumulated at the interface and realize uniform deposition of sodium at the interface. In addition, the addition of 1% to 10% of the conductive agent can increase the amorphous region of the polymer matrix to a certain extent and increase the diffusion rate of sodium ions in the solid electrolyte layer. The conductive agent can be a non-ionic conductor. In some embodiments, the amount of the conductive agent added can be a combination of 2% to 9%, 3% to 8%, 4% to 7%, 5% to 6% or more.
[0039] In some embodiments, the mass percentage of each component in the first composite solid electrolyte layer in the first composite solid electrolyte layer can be: 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler, 0.5% to 20% of the plasticizer, and the molar ratio of the sodium ions in the sodium salt to the polymer monomers in the polymer matrix can be (0 to 1): 20. For example, it can include 30% to 70% of the polymer matrix, 12% to 60% of the inorganic filler, and 4% to 17% of the plasticizer; or it can include 32% to 68% of the polymer matrix, 20% to 56% of the inorganic filler, 7% to 15% of the plasticizer, or a combination of the above ranges. The molar ratio of the sodium ions in the sodium salt to the polymer monomers in the polymer matrix can be 0.3:20, or 0.5:20, or 0.8:20, or a combination of the above ranges.
[0040] In some embodiments, the mass percentage of each component in the second composite solid electrolyte layer can be: 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler, 0.5% to 20% of the plasticizer and 1% to 10% of the conductive agent.
[0041] Since the simple polymer solid electrolyte has low ionic conductivity, poor thermal stability and poor performance in inhibiting the growth of sodium dendrites on the negative electrode side, on the contrary, the inorganic filler has high ionic conductivity, good thermal stability and has a certain inhibitory effect on the growth of dendrites on the negative electrode side, but the inorganic solid electrolyte is not easy to process and has poor interface contact, therefore, the polymer matrix and the inorganic filler need to have a relationship in terms of dosage. The present invention sets the dosage of the polymer matrix and the inorganic filler in the first composite solid electrolyte layer and the second composite solid electrolyte layer within the above range, so that the solid electrolyte has good ionic conductivity and thermal stability, has a certain inhibitory effect on the growth of sodium dendrites on the negative electrode side and is convenient for the processing of the electrolyte. The molar ratio of sodium salt to polymer monomer is set to (0-1):20, which can improve the ionic conductivity of the composite solid electrolyte without reducing the film-forming performance of the composite solid electrolyte.
[0042] It is understandable that, in some embodiments, in the first composite solid electrolyte layer and the second composite solid electrolyte layer disclosed herein, there may be no inorganic filler (i.e., the mass proportion may be 0%). The addition of inorganic fillers can increase the mechanical strength and ionic conductivity of the diaphragm, but does not affect the preparation process of the asymmetric composite membrane. In other words, even if the first composite solid electrolyte layer and the second composite solid electrolyte layer do not contain inorganic fillers, they can solve the technical problems of the present application and achieve the technical effects of the present application. However, the absence of inorganic fillers may cause the ionic conductivity of the composite solid electrolyte diaphragm to be somewhat low; the addition of inorganic fillers only makes the performance of the first composite solid electrolyte layer and the second composite solid electrolyte layer disclosed herein better.
[0043] It is understandable that, in some embodiments, in the first composite solid electrolyte layer and the second composite solid electrolyte layer disclosed herein, there may be no plasticizer (i.e., the mass percentage may be 0%). The role of the plasticizer in the present disclosure is to increase the layer film of the polymer matrix during the process, so that the polymer, sodium salt, etc. in the composite film are evenly dispersed, and it can also increase the ionic conductivity of the composite film to a certain extent. In other words, even if the first composite solid electrolyte layer and the second composite solid electrolyte layer do not contain plasticizers, they can solve the technical problems of the present application and achieve the technical effects of the present application. The addition of plasticizers only makes the performance of the first composite solid electrolyte layer and the second composite solid electrolyte layer disclosed herein better.
[0044] For example, the content ratio of each component in the second composite solid electrolyte layer can be: 20% to 85% polymer matrix, 5% to 70% inorganic filler, 4% to 17% plasticizer and 1% to 8% conductive agent; or 22% to 80% polymer matrix, 7% to 65% inorganic filler, 5% to 12% plasticizer and 3% to 6% conductive agent, or a combination of the above ranges. The molar ratio of sodium salt to polymer monomer can be (0 to 1): 20. The molar ratio of sodium salt to polymer monomer can also be 0.3:20, or 0.5:20, or 0.7:20, or 0.9:20 or a combination of the above ranges.
[0045] In some embodiments, the mass ratio of the first composite solid electrolyte layer to the second composite solid electrolyte layer may be (1-8): 1. For example, the mass ratio of the first composite solid electrolyte layer to the second composite solid electrolyte layer may be 3:1, 5:1, 6:1, 7:1 or a combination of the above ranges.
[0046] In some embodiments, the thickness of the second composite solid electrolyte layer may be 0.1 mm to 1 mm. Setting the thickness of the second composite solid electrolyte layer within the above range can reduce the cost of using the conductive agent while ensuring that the composite solid electrolyte has good performance. For example, the thickness of the second composite solid electrolyte layer may be 0.2 mm or 0.5 mm.
[0047] In some embodiments, the polymer matrix in the first composite solid electrolyte layer and the second composite solid electrolyte layer can be one or a combination of polyethylene oxide (PEO), polyacrylonitrile (PAN), poly(methyl methacrylate) (PMMA), poly(vinyl alcohol) (PVA), polyvinyl pyrrolidone (PVP), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polypropylene carbonate (PPC), and polyvinyl carbonate (PEC).
[0048] In some embodiments, the inorganic filler in the first composite solid electrolyte layer and the second composite solid electrolyte layer can be Si, Al2O3, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+x Zr2Si x P 3-x O 12 (0≤x≤3) and NaMM′P3O 12 One or more combinations of, wherein M and M' can be Si 2+ Mg 2+ , Cu 2+ 、Co 2+ 、Zn 2+ , Mn 2+ , Fe 2+ 、Al 3 + Cr 3+ Sc 3+ , Y 3+ ,La 3+ 、Ti 4+ 、Zr 4+ ,Ge 4+ Sn 4+ , Nb 4+ 、V 5+ , Nb 5+ and Ta 5+ In any one of the above, M and M' may be the same or different.
[0049] In some embodiments, the sodium salt in the first composite solid electrolyte layer and the second composite solid electrolyte layer can be one or a combination of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI and sodium bis(oxalatoborate).
[0050] In some embodiments, the plasticizer in the first composite solid electrolyte layer and the second composite solid electrolyte layer can be one or a combination of several of succinonitrile, polystyrene, ethylene carbonate, propylene carbonate, polyethylene glycol, polyethylene glycol dimethyl ether, tetraethylene glycol, triethylene glycol dimethyl ether, diethyl phthalate, dioctyl phthalate, cyclic phosphate ester, dibutyl phthalate and dimethyl phthalate.
[0051] In some embodiments, the conductive agent in the second composite solid electrolyte layer may be one or a combination of graphite, graphene, carbon nanotubes, acetylene black and Ketjen black.
[0052] In some embodiments, the asymmetric laminated sodium-based composite solid electrolyte provided by the present invention can be used as a diaphragm material for sodium-ion batteries, and is an asymmetric laminated sodium-based diaphragm material.
[0053] Another aspect of the present invention provides a method for preparing an asymmetric laminated sodium-based composite solid electrolyte. In some embodiments, the preparation method may include the following steps:
[0054] S01, mixing a polymer matrix, an inorganic filler, a sodium salt, a plasticizer and an organic solvent to obtain a first composite solid electrolyte slurry
[0055] S02, applying the first composite solid electrolyte slurry to a mold by scraping, and drying with air to obtain a first composite solid electrolyte layer;
[0056] S03, mixing a polymer matrix, an inorganic filler, a sodium salt, a plasticizer, a conductive agent and an organic solvent to obtain a second composite solid electrolyte slurry;
[0057] S04, coating the second composite solid electrolyte slurry on the first composite solid electrolyte layer, first drying by air blast, and then drying by vacuum to obtain an asymmetric laminated sodium-based composite solid electrolyte.
[0058] In some embodiments, the content of the raw materials added in the above preparation method is adapted to the content of the components contained in the above-mentioned asymmetric laminated sodium-based composite solid electrolyte, that is, the first composite solid electrolyte includes 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler, and 0.5% to 20% of the plasticizer by mass percentage, and the molar ratio of the sodium salt to the polymer monomer can be (0 to 1): 20. The second composite solid electrolyte includes 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler, 0.5% to 20% of the plasticizer, and 1% to 10% of the conductive agent by mass percentage, which will not be repeated here.
[0059] In some embodiments, the organic solvent in the first composite solid electrolyte slurry and the second composite solid electrolyte slurry is one or a combination of acetone, N,N-dimethylformyl and nitrogen methyl pyrrolidone; or, the organic solvent can be a mixture of acetone and N,N-dimethylformyl in a mass ratio of (1 to 25):1; or, the organic solvent can be a mixture of acetone and nitrogen methyl pyrrolidone in a mass ratio of (1 to 25):1. For example, the organic solvent can be a mixture of acetone and N,N-dimethylformyl in a mass ratio of 15:1; or, the organic solvent can be a mixture of acetone and nitrogen methyl pyrrolidone in a mass ratio of 18:1.
[0060] In some embodiments, the mass percentage of the organic solvent in the first composite solid electrolyte slurry may be 67% to 83%. For example, the mass percentage may be 70%, 75%, 79%, 81% or a combination thereof.
[0061] In some embodiments, the mass percentage of the organic solvent in the second composite solid electrolyte slurry may be 67% to 83%. For example, the mass percentage may be 70%, 72%, 75%, 79%, 81% or a combination thereof.
[0062] In some embodiments, the first composite solid electrolyte slurry can be obtained after magnetic stirring at 25° C. to 60° C. for 6 h to 18 h. For example, the first composite solid electrolyte slurry can be obtained after magnetic stirring at 45° C. for 12 h.
[0063] In some embodiments, the second composite solid electrolyte slurry can be obtained after magnetic stirring at 25° C. to 60° C. for 6 h to 18 h. For example, the second composite solid electrolyte slurry can be obtained after magnetic stirring at 52° C. for 14 h.
[0064] In some embodiments, the mold may be a polytetrafluoroethylene mold. The groove depth of the mold may be 0.1 mm to 1 mm. For example, the groove depth of the mold may be 0.5 mm.
[0065] In some embodiments, the first composite solid electrolyte slurry can be coated on a polytetrafluoroethylene mold by a doctor blade method, and the blast drying temperature can be 25° C. to 80° C., and the drying time can be 20 min to 120 min. For example, the blast drying temperature can be 60° C., and the drying time can be 50 min.
[0066] In some embodiments, the mass ratio of the first composite solid electrolyte slurry to the second composite solid electrolyte slurry may be (1-8): 1. For example, the mass ratio may be 5:1.
[0067] In some embodiments, after the second composite solid electrolyte slurry is poured and coated, the blast drying temperature may be 25°C to 80°C, the drying time may be 30min to 180min, the vacuum drying temperature may be 45°C to 80°C, and the drying time may be 12h to 36h. For example, the blast drying temperature may be 55°C, the blast drying time may be 120min, the vacuum drying temperature may be 65°C, and the vacuum drying time may be 20h.
[0068] Another aspect of the present invention provides a sodium ion battery. In some embodiments, the sodium ion battery includes the asymmetric laminated sodium-based composite solid electrolyte described above. The asymmetric laminated sodium-based composite solid electrolyte is disposed between the positive electrode and the negative electrode. Figure 4 As shown, the sodium ion battery includes a current collector 40, a positive electrode 41, a negative electrode 42, a first composite solid electrolyte layer 43 connected to the positive electrode 41, and a second composite solid electrolyte layer 44 disposed between the negative electrode 42 and the first composite solid electrolyte layer 43.
[0069] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.
[0070] Example 1
[0071] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PEO, 0.14 g diethyl phthalate, 0.01 g NaFSI, 3 g acetone and 2.5 g N,N-dimethylformamide were mixed and magnetically stirred at 50 °C for 3 h to obtain a transparent solution; 0.45 g Na3Zr2Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 50° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0072] Similarly, 0.81 g PEO, 0.14 g diethyl phthalate, 0.01 g NaFSI, 3 g acetone and 2.5 g N,N-dimethylformamide were mixed in a glove box and magnetically stirred at 50 °C for 3 h to obtain a transparent solution; 0.54 g Na3Zr2Si2PO 12 The powder and 0.04 g of graphite were added to the above solution, and the solution was magnetically stirred at a constant temperature of 50° C. for 18 h to obtain a second composite solid electrolyte slurry.
[0073] Step 2: Take the first composite solid electrolyte slurry out of the glove box, slowly pour it in a small coating machine and apply it to a polytetrafluoroethylene mold with an inner groove size of 160×70×0.5 mm, and dry it with air at 45°C for 30 minutes to obtain the first composite solid electrolyte layer, the SEM image of which is as follows: Figure 1 The second composite solid electrolyte slurry was taken out of the glove box, slowly coated on the first composite solid electrolyte layer by scraping, and dried at 50°C for 60 minutes. A second composite solid electrolyte layer was formed on the first composite solid electrolyte layer. The SEM image of the second composite solid electrolyte layer is shown in FIG. Figure 2 shown.
[0074] The laminated composite solid electrolyte was removed from the polytetrafluoroethylene mold and vacuum dried at 60° C. for 24 h to obtain an asymmetric laminated sodium-based composite solid electrolyte.
[0075] The cross-sectional SEM image of the asymmetric laminated sodium-based composite solid electrolyte obtained above is as follows: Figure 3 As shown in the figure, the characterization results show that it has a uniform planar structure and the layers are strongly bonded and do not separate. Through testing, the sodium ion conductivity of the asymmetric laminated sodium-based composite solid electrolyte is 2.13×10 -4 S cm -1 .
[0076] Step 3: Cut the laminated composite solid electrolyte into φ19mm discs as the battery's diaphragm and solid electrolyte, and assemble a CR2032-type button-type Na||Na symmetrical battery by soaking the electrode and solid electrolyte interface with electrolyte. Figure 4 The structure of the sodium ion battery with asymmetric composite solid electrolyte is shown; at 0.1 mA cm -1 Conduct stability tests according to Figure 5 The symmetrical battery charge / discharge cycle performance is shown; the CR2032 button type is assembled with Na3V2(PO4)3 positive electrode active material, and its electrochemical performance is tested under 0.1C conditions and 2.3~3.8V voltage range. Figure 7 The first cycle charge and discharge performance of Na||Na3V2(PO4)3 battery (CR2032 button type) is shown.
[0077] Example 2
[0078] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PEO, 0.27 g dimethyl phthalate, 0.07 g NaClO4, 3.2 g acetone and 2.5 g N,N-dimethylformamide were mixed and stirred at 40 °C for 3 h to obtain a transparent solution; 0.63 g Na 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 40° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0079] Similarly, 0.81 g PEO, 0.27 g dimethyl phthalate, 0.07 g NaClO4, 3.2 g acetone and 2.5 g N,N-dimethylformamide were mixed in a glove box and magnetically stirred at 40 °C for 3 h to obtain a transparent solution; 0.63 g Na 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder and 0.04 g of graphite were added to the above solution, and magnetic stirring was performed at a constant temperature of 40° C. for 18 h to obtain a second composite solid electrolyte slurry.
[0080] The subsequent operations are the same as step 2 and step 3 in Example 1. The sodium ion conductivity of the asymmetric laminated sodium-based composite solid electrolyte prepared in this example is 2.16×10 -4 S cm -1 .according to Figure 7 The first cycle charge and discharge performance of Na||Na3V2(PO4)3 battery is shown. Figure 8 The rate performance of Na||Na3V2(PO4)3 battery (CR2032 type button type) is shown.
[0081] Example 3
[0082] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PEO, 0.14 g tetraethylene glycol, 0.01 g NaClO4 and 5.5 g N,N-dimethylformamide were mixed and stirred at 45 °C for 3 h to obtain a transparent solution; 0.54 g Na3Zr2Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 45° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0083] Similarly, 0.81 g PEO, 0.14 g tetraethylene glycol, 0.07 g NaClO4 and 5.5 g N,N-dimethylformamide were mixed in a glove box and magnetically stirred at 45 °C for 3 h to obtain a transparent solution; 0.54 g Na3Zr2Si2PO 12 The powder and 0.08 g of acetylene black were added to the above solution, and the solution was magnetically stirred at a constant temperature of 45° C. for 18 h to obtain a second composite solid electrolyte slurry.
[0084] The subsequent operations are the same as step 2 and step 3 of Example 1. The sodium ion conductivity of the asymmetric laminated sodium-based composite solid electrolyte prepared in this example is 1.98×10 -4 S cm -1 .according to Figure 8 The first cycle charge and discharge performance of Na||Na3V2(PO4)3 battery (CR2032 button type) is shown.
[0085] Example 4
[0086] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.59 g PEO, 0.14 g dibutyl phthalate, 0.01 g NaFSI, 3 g acetone and 4 g N,N-dimethylformamide were mixed and stirred at 45 °C for 3 h to obtain a transparent solution; 1.08 g Na 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 45° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0087] Similarly, 0.59 g PEO, 0.135 g dibutyl phthalate, 0.01 g NaFSI, 3 g acetone and 4 g N,N-dimethylformamide were mixed in a glove box and magnetically stirred at 45 °C for 3 h to obtain a transparent solution. 1.08 g Na 3.4 Zr 1.8 Mg 0.2Si2PO 12 The powder and 0.08 g of graphite were added to the above solution, and magnetic stirring was performed at a constant temperature of 45° C. for 18 h to obtain a second composite solid electrolyte slurry.
[0088] The subsequent operations are the same as step 2 and step 3 of Example 1. The sodium ion conductivity of the asymmetric laminated sodium-based composite solid electrolyte prepared in this example is 2.27×10 -4 S cm -1 .
[0089] Example 5
[0090] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.59 g PEO, 0.14 g tetraethylene glycol, 0.01 g NaClO4, 3 g acetone and 3.3 g N,N-dimethylformamide were mixed and stirred at 45 °C for 3 h to obtain a transparent solution; 1.08 g Na3Zr2Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 45° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0091] Similarly, 0.59 g PVDF-HFP, 0.135 g tetraethylene glycol, 0.01 g NaClO4, 3 g acetone and 3.3 g N,N-dimethylformamide were mixed in a glove box and magnetically stirred at 45 °C for 3 h to obtain a transparent solution; 1.08 g Na3Zr2Si2PO 12 The powder and 0.08 g of graphene were added to the above solution, and magnetic stirring was performed at a constant temperature of 45° C. for 18 h to obtain a second composite solid electrolyte slurry.
[0092] The subsequent operations are the same as step 2 and step 3 of Example 1. The sodium ion conductivity of the asymmetric laminated sodium-based composite solid electrolyte prepared in this example is 2.58×10 -4 S cm -1 .
[0093] Comparative Example 1
[0094] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PEO, 0.14 g tetraethylene glycol, 0.01 g NaClO4, 3 g acetone and 3.5 g N,N-dimethylformamide were mixed and stirred at 45 °C for 3 h to obtain a transparent solution; 0.54 g Na3Zr2Si2PO 12 The powder was added to the above solution and magnetically stirred at 45° C. for 18 h to obtain a first composite solid electrolyte slurry. Similarly, the second composite solid electrolyte slurry was the same as the first composite solid electrolyte slurry, that is, compared with Example 1, no conductive agent was added to the second composite solid electrolyte slurry.
[0095] The subsequent operations are the same as step 2 and step 3 of Example 1. The sodium ion conductivity of the composite solid electrolyte obtained above is 1.53×10 -4 S cm -1 .according to Figure 6 The charge / discharge cycle performance of the Na||Na symmetric battery is shown. Figure 7 The first cycle charge and discharge performance of Na||Na3V2(PO4)3 battery (CR2032 button type) is shown.
[0096] Comparative Example 2
[0097] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 8.1 g of PEO, 0.27 g of dibutyl phthalate, 0.07 g of NaClO4, 3 g of acetone and 2.5 g of N,N-dimethylformamide were mixed and stirred at 45 °C for 3 h to obtain a transparent solution; 0.72 g of Na 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder was added into the above solution, and the solution was magnetically stirred at a constant temperature of 45° C. for 18 h to obtain the first composite solid electrolyte slurry.
[0098] Similarly, 0.81 g PEO, 0.27 g dibutyl phthalate, 0.07 g NaClO4, 3.5 g acetone and 2.5 g N,N-dimethylformamide were mixed in a glove box and stirred at 45 °C for 3 h to obtain a transparent solution. 3.4 Zr 1.8 Mg 0.2 Si2PO 12 The powder was added to the above solution, and magnetic stirring was performed at a constant temperature of 45° C. for 18 h to obtain a second composite solid electrolyte slurry. That is, compared with Example 2, no conductive agent was added to the second composite solid electrolyte slurry.
[0099] The subsequent operations are the same as step 2 and step 3 of Example 1. The sodium ion conductivity of the composite solid electrolyte obtained above is 1.37×10 -4 S cm -1 .
[0100] Comparative Example 3
[0101] Step 1: In a glove box with an argon atmosphere and a water content of ≤0.1 ppm, 0.81 g PEO, 0.135 g diethyl phthalate, 0.01 g NaFSI, 3 g acetone and 2.5 g N,N-dimethylformamide were mixed and magnetically stirred at 45 °C for 3 h to obtain a transparent solution; 0.63 g Na3Zr2Si2PO 12The powder was added to the above solution and magnetically stirred at a constant temperature of 45° C. for 18 h to obtain a solid electrolyte slurry.
[0102] Step 2: Take the above solid electrolyte slurry out of the glove box, slowly pour and scrape it into a polytetrafluoroethylene mold with an inner groove size of 160×70×0.5 mm in a constant temperature drying small coating machine, dry it with air at 60°C for 120 minutes, remove the composite solid electrolyte from the polytetrafluoroethylene mold, and vacuum dry it at 60°C for 24 hours to obtain a single-layer composite solid electrolyte.
[0103] The subsequent operation is the same as step 3 of Example 1. The sodium ion conductivity of the composite solid electrolyte is 1.34×10 -4 S cm -1 That is, compared with Example 3, this comparative example does not have a second composite solid electrolyte layer.
[0104] The results of Examples 1-5 and Comparative Examples 1-3 are compared as shown in the following table. It can be seen from Table 1 that the first charge specific capacity of the Na||Na3V2(PO4)3 battery (CR2032 button type) corresponding to the asymmetric laminated composite solid electrolyte prepared by the present invention at 0.1C is significantly higher than that of the single-layer composite solid electrolyte and the symmetrical laminated composite solid electrolyte (the first composite solid electrolyte slurry and the second composite solid electrolyte slurry have the same composition); the charge and discharge cycle stability of the Na||Na symmetric battery (CR2032 button type) corresponding to the asymmetric laminated sodium-based composite solid electrolyte is significantly better than that of the symmetrical laminated composite solid electrolyte, indicating that the asymmetric laminated sodium-based composite solid electrolyte prepared by the present invention has good sodium ion conductivity and electrochemical stability.
[0105]
[0106] Figure 4 The Na-Na symmetric battery charge and discharge cycle curve corresponding to the composite solid electrolyte prepared in Example 1 of the present invention is shown. Figure 5 The charge-discharge cycle curve of the Na-Na symmetric battery corresponding to the composite solid electrolyte prepared in Comparative Example 1 is shown. Figure 4 and Figure 5 It can be seen that the asymmetric layered sodium-based composite solid electrolyte has good cycling stability for sodium-ion batteries.
[0107] Figure 6 The first cycle charge and discharge curves of Na||Na3V2(PO4)3 battery (CR2032 button type) corresponding to the composite solid electrolyte prepared in Example 1 of the present invention and Comparative Example 1 are shown. Figure 7The first cycle charge and discharge curves of Na||Na3V2(PO4)3 battery (CR2032 button type) corresponding to the composite solid electrolyte prepared in Example 2 and Example 3 of the present invention are shown. Figure 6 and Figure 7 It can be seen that the first-cycle specific capacity of the sodium-ion battery corresponding to the asymmetric stacked sodium-based composite solid electrolyte is better than that of the symmetric stacked sodium-based composite solid electrolyte.
[0108] Fig. 9 The rate performance curves of Na||Na3V2(PO4)3 batteries (CR2032 button type) corresponding to the composite solid electrolytes prepared in Example 2 and Comparative Example 2 of the present invention are shown. Fig. 9 It can be seen that the sodium-ion battery corresponding to the asymmetric stacked sodium-based composite solid electrolyte has better rate performance.
[0109] Although the present invention has been described above by combining with exemplary embodiments, it will be apparent to those skilled in the art that various modifications and changes may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.
Claims
1. An asymmetric laminated sodium-based composite solid electrolyte, characterized in that: The invention comprises a first composite solid electrolyte layer adjacent to the positive electrode of the battery, and a second composite solid electrolyte layer arranged between the first composite solid electrolyte layer and the negative electrode of the battery, wherein: The first composite solid electrolyte layer comprises a polymer matrix and a sodium salt; The second composite solid electrolyte layer comprises a polymer matrix, a sodium salt and a conductive agent, wherein the conductive agent accounts for 1% to 10% of the mass of the second composite solid electrolyte layer.
2. The asymmetric layered sodium-based composite solid electrolyte according to claim 1, characterized in that: The first composite solid electrolyte layer also contains inorganic fillers, wherein the mass percentage of each component in the first composite solid electrolyte layer is: 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler; the molar ratio of the sodium ions in the sodium salt to the polymer monomers in the polymer matrix is (0 to 1):
20.
3. The asymmetric layered sodium-based composite solid electrolyte according to claim 1, characterized in that: The second composite solid electrolyte layer also contains inorganic fillers, wherein the mass percentage of each component in the second composite solid electrolyte layer is: 15% to 95% of the polymer matrix, 0.5% to 70% of the inorganic filler; the molar ratio of the sodium ions in the sodium salt to the polymer monomers in the polymer matrix is (0 to 1):
20.
4. The asymmetric layered sodium-based composite solid electrolyte according to claim 1, 2 or 3, characterized in that: The first composite solid electrolyte layer further includes a plasticizer, wherein the mass percentage of the plasticizer in the first composite solid electrolyte layer is 0.5% to 20%; The second composite solid electrolyte layer also includes a plasticizer, and the mass percentage of the plasticizer in the second composite solid electrolyte layer is 0.5% to 20%.
5. The asymmetric layered sodium-based composite solid electrolyte according to claim 1, 2 or 3, characterized in that: The mass ratio of the first composite solid electrolyte layer to the second composite solid electrolyte layer is (1-8):
1.
6. The asymmetric layered sodium-based composite solid electrolyte according to claim 1, 2 or 3, characterized in that: The polymer matrix is selected from at least one of polyethylene oxide, polyacrylonitrile, poly(methyl methacrylate), poly(vinyl alcohol), polyvinyl pyrrolidone, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene), polypropylene carbonate and polyvinyl carbonate; Inorganic fillers are selected from Si, Al2O3, AlCl3, BaTiO3, CuO, SiO2, ZrO2, TiO2, Na 1+x Zr2Si x P 3-x O 12 and NaMM′P3O 12 At least one of, wherein 0≤x≤3, M and M′ are Si 2+ Mg 2+ , Cu 2+ 、Co 2+ 、Zn 2+ , Mn 2+ , Fe 2+ 、Al 3+ Cr 3+ Sc 3+ , Y 3+ ,La 3+ 、Ti 4+ 、Zr 4+ ,Ge 4+ Sn 4+ , Nb 4+ 、V 5+ , Nb 5+ and Ta 5+ In any of the above, M and M' are the same or different; The sodium salt is selected from at least one of NaClO4, NaPF6, NaAsF6, NaBF4, NaTFSI, NaTf, NaFSI and sodium bis(oxalatoborate); The plasticizer is selected from at least one of succinonitrile, polystyrene, ethylene carbonate, propylene carbonate, polyethylene glycol, polyethylene glycol dimethyl ether, tetraethylene glycol, triethylene glycol dimethyl ether, diethyl phthalate, dioctyl phthalate, cyclic phosphate, dibutyl phthalate and dimethyl phthalate; The conductive agent is selected from at least one of graphite, graphene, carbon nanotubes, acetylene black and Ketjen black.
7. A method for preparing an asymmetric laminated sodium-based composite solid electrolyte, characterized in that: The following steps are involved: The polymer matrix, the inorganic filler, the sodium salt, the plasticizer and the organic solvent are mixed to obtain a first composite solid electrolyte slurry; Applying the first composite solid electrolyte slurry on the mold by knife coating and drying with air blast to obtain a first composite solid electrolyte layer; The polymer matrix, the inorganic filler, the sodium salt, the plasticizer, the conductive agent and the organic solvent are mixed to obtain a second composite solid electrolyte slurry; The second composite solid electrolyte slurry is coated on the first composite solid electrolyte layer, and then air-dried and vacuum-dried to obtain an asymmetric laminated sodium-based composite solid electrolyte.
8. The method for preparing an asymmetric laminated sodium-based composite solid electrolyte according to claim 7, characterized in that: The organic solvent in the first composite solid electrolyte slurry and the second composite solid electrolyte slurry is one or a combination of acetone, N,N-dimethylformyl and nitrogen methyl pyrrolidone; Alternatively, the organic solvent is a mixture of acetone and N,N-dimethylformyl in a mass ratio of (1-25):1; Alternatively, the organic solvent is a mixed solution of acetone and nitrogen methyl pyrrolidone in a mass ratio of (1-25):
1.
9. The method for preparing an asymmetric laminated sodium-based composite solid electrolyte according to claim 7, characterized in that: The first composite solid electrolyte slurry is coated on a polytetrafluoroethylene mold by a blade coating method, and the blast drying temperature is 25°C to 80°C, and the drying time is 20min to 120min. After the second composite solid electrolyte slurry is coated, the blast drying temperature is 25°C to 80°C, the drying time is 30min to 180min, and the vacuum drying temperature is 45°C to 80°C, and the drying time is 12h to 36h.
10. A sodium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an asymmetric layered sodium-based composite solid electrolyte as claimed in any one of claims 1 to 6 located between the positive electrode and the negative electrode.