All-solid-state battery

By using a solid electrolyte with a γ-Li3PO4 crystal structure and Ag or Ag alloy as the negative active material in an all-solid-state battery, the sintered body structure is optimized, which solves the problem of low energy density of existing all-solid-state batteries and achieves high energy density and Increase in output voltage.

CN118749146APending Publication Date: 2024-10-08TDK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092562.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-28
Filing Date
2022-09-30
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing all-solid-state batteries have small output voltage and low energy density.

Method used

The first and second solid electrolytes with γ-Li3PO4 type crystal structure are used, combined with Ag or Ag alloy as the negative electrode active material, and the sintered body structure is optimized to ensure that the volume ratio between the solid electrolyte layer and the negative electrode is above 5%55 % or less, the volume ratio of Ag or Ag alloy is between 45% and below 95%, forming an all-solid-state battery with high energy density.

Benefits of technology

The energy density of all-solid-state batteries is significantly improved. The Ag and Ag alloy in the negative electrode act as active materials, increasing the potential difference and improving the output voltage and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749146A_ABST
    Figure CN118749146A_ABST
Patent Text Reader

Abstract

An all-solid-state battery provided with a sintered body having a positive electrode, a negative electrode, and a solid electrolyte layer positioned between the positive electrode and the negative electrode, the solid electrolyte layer having a first solid electrolyte having a gamma-Li3PO4-type crystal structure, the negative electrode has: a second solid electrolyte having a gamma-Li3PO4-type crystal structure; and at least one type selected from the group consisting of Ag and an alloy containing Ag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an all-solid-state battery.

[0002] This application claims priority based on Japanese Patent Application No. 2022-028957 filed in Japan on February 28, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In recent years, electronic technology has developed significantly, achieving small, light, thin, and multifunctional portable electronic devices. As a result, there is a strong demand for batteries that serve as power sources for electronic devices to be small, light, thin, and have improved reliability, and all-solid-state batteries using solid electrolytes as electrolytes have attracted much attention.

[0004] All-solid batteries include thin-film type and bulk type. Thin-film type can be made using thin-film technology such as physical vapor deposition (PVD) and sol-gel method. Bulk type can be made using powder forming method, sintering method, etc. Due to different manufacturing methods, different all-solid batteries can be used with different materials and have different performances.

[0005] For example, sintered all-solid batteries using an oxide-based solid electrolyte as a solid electrolyte are disclosed in Patent Documents 1 and 2. Patent Documents 1 and 2 describe examples in which titanium oxide is used as a negative electrode active material layer.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: International Publication No. 2007 / 135790

[0009] Patent Document 2: International Publication No. 2008 / 099508 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] The all-solid-state batteries described in Patent Documents 1 and 2 have low output voltages and low energy densities.

[0012] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide an all-solid-state battery having a high energy density.

[0013] Means for solving technical problems

[0014] In order to solve the above technical problems, the following means are provided.

[0015] (1) A first embodiment of an all-solid-state battery comprises a sintered body having a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode, wherein the solid electrolyte layer has a first solid electrolyte having a γ-Li3PO4 type crystal structure, and the negative electrode has a second solid electrolyte and one or more selected from Ag and an alloy containing Ag, wherein the second solid electrolyte has a γ-Li3PO4 type crystal structure.

[0016] (2) In the all-solid-state battery of the above aspect, the volume ratio of the second solid electrolyte to the entire negative electrode may be 5% to 55%.

[0017] (3) In the all-solid-state battery of the above embodiment, the first solid electrolyte may include Li 3+x Si x P 1-x O4(0.2≤x≤0.6).

[0018] (4) In the all-solid-state battery of the above embodiment, the second solid electrolyte may include Li 3+x Si x P 1-x O4(0.2≤x≤0.6).

[0019] (5) In the all-solid-state battery of the above aspect, the first solid electrolyte and the second solid electrolyte may have the same constituent elements.

[0020] (6) In the all-solid-state battery of the above aspect, the volume ratio of the Ag or Ag alloy to the entire negative electrode may be 45% to 95%.

[0021] (7) In the all-solid-state battery of the above embodiment, the sum of the volume ratio of the solid electrolyte to the entire negative electrode and the volume ratio of the Ag or Ag alloy to the entire negative electrode may be 95% to 100%.

[0022] (8) In the all-solid-state battery of the above aspect, the alloy containing Ag may be a Li—Ag alloy.

[0023] (9) In the all-solid-state battery of the above aspect, the positive electrode may include lithium cobalt oxide.

[0024] (10) In the all-solid-state battery of the above aspect, the positive electrode may include a current collector layer containing Ag and a positive electrode active material layer in contact with at least one main surface of the current collector layer.

[0025] Effects of the Invention

[0026] The all-solid-state battery of the above type has a high energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a cross-sectional view of the all-solid-state battery according to the first embodiment.

[0028] Figure 2 This is an enlarged cross-sectional view of a characteristic portion of the all-solid-state battery according to the first embodiment.

[0029] Figure 3 This is an enlarged cross-sectional view of a characteristic portion of another example of the all-solid-state battery of the first embodiment.

[0030] Figure 4 This is an enlarged cross-sectional view of a characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment.

[0031] Figure 5 This is an enlarged cross-sectional view of a characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment.

[0032] Explanation of symbols

[0033] 1… Positive electrode

[0034] 1A, 1C, 1D, 1E...Positive electrode collector layer

[0035] 1B……Positive electrode active material layer

[0036] 1F…Middle floor

[0037] 2……Negative electrode

[0038] 3…Solid electrolyte layer

[0039] 4...Laminated

[0040] 5, 6...Terminal electrodes

[0041] 10…All-solid-state batteries

[0042] 11, 21……Current collector

[0043] 12……Positive electrode active material

[0044] 13...Oxide

[0045] 22…The second solid electrolyte DETAILED DESCRIPTION

[0046] Hereinafter, the present embodiment will be described in detail with reference to the drawings as appropriate. In order to facilitate understanding of the features of the present invention, the drawings used in the following description sometimes enlarge the features for convenience, and sometimes the dimensional ratios of the components are different from the actual ones. The materials, dimensions, etc. illustrated in the following description are only examples, and the present invention is not limited to these, and can be implemented by appropriate changes within the scope of the purpose.

[0047] Directions are defined. The stacking direction of the stacked body 4 is set to the z direction, a direction in a plane perpendicular to the z direction is set to the x direction, and a direction perpendicular to the x direction and the z direction is set to the y direction. Hereinafter, a direction in the z direction is sometimes expressed as "up", and the direction opposite to the direction is sometimes expressed as "down". Up and down are not necessarily consistent with the direction in which gravity is applied.

[0048] Figure 1 Schematic cross-sectional view of the all-solid battery 10 of the present embodiment. The all-solid battery 10 has a stack 4 and terminal electrodes 5, 6. The terminal electrodes 5, 6 are in contact with the opposite surfaces of the stack 4. The terminal electrodes 5, 6 extend in the z direction intersecting (orthogonal) with the stacking surface of the stack 4.

[0049] The laminate 4 has a positive electrode 1, a negative electrode 2, and a solid electrolyte layer 3. The laminate 4 is a sintered body obtained by laminating the positive electrode 1, the negative electrode 2, and the solid electrolyte layer 3 and sintering them. The number of layers of the positive electrode 1 and the negative electrode 2 is not particularly limited. The solid electrolyte layer 3 is at least between the positive electrode 1 and the negative electrode 2. Between the positive electrode 1 and the terminal electrode 6 and between the negative electrode 2 and the terminal electrode 5, for example, there is a solid electrolyte that is the same as that of the solid electrolyte layer 3. One end of the positive electrode 1 is connected to the terminal electrode 5. One end of the negative electrode 2 is connected to the terminal electrode 6.

[0050] The all-solid-state battery 10 is charged or discharged by transfer of ions between the positive electrode 1 and the negative electrode 2 via the solid electrolyte layer 3. Figure 1 A stacked battery is shown in FIG. 1 , but a wound battery may also be used. The all-solid battery 10 is used, for example, for a laminate battery, a square battery, a cylindrical battery, a coin battery, a button battery, etc. In addition, the all-solid battery 10 may also be a liquid injection type in which the solid electrolyte layer 3 is dissolved or dispersed in a solvent.

[0051] "positive electrode"

[0052] Figure 2 This is an enlarged view of a characteristic portion of the all-solid-state battery 10 of the first embodiment. The positive electrode 1 has, for example, a positive electrode collector layer 1A and a positive electrode active material layer 1B. The positive electrode has, for example, a collector layer containing Ag and a positive electrode active material layer in contact with at least one main surface of the collector layer.

[0053] [Positive electrode current collector layer]

[0054] The positive electrode current collector layer 1A includes, for example, a current collector 11 and a positive electrode active material 12. In this case, the area between the xy plane passing through the uppermost portion of the current collector 11 and the xy plane passing through the lowermost portion is regarded as the positive electrode current collector layer 1A.

[0055] The current collector 11 is composed of a plurality of current collector particles. The plurality of current collector particles are connected to each other and are electrically connected in the xy plane. In the positive electrode 1, the current collector 11 includes a metal or alloy selected from any one of Ag, Pd, Au, and Pt. Even when the stack 4 is heated in an atmospheric atmosphere, these metals or alloys do not melt and are difficult to oxidize. The current collector 11 is, for example, an AgPd alloy, Au, or Pt.

[0056] The positive electrode active material 12 is mixed with the current collector 11 and exists in the positive electrode current collector layer 1A. The positive electrode active material 12 is in contact with the current collector 11. When the positive electrode active material 12 is contained in the positive electrode current collector layer 1A, the transfer of electrons from the positive electrode active material 12 to the current collector 11 becomes smooth. The positive electrode active material 12 is the same as the material contained in the positive electrode active material layer 1B described later.

[0057] exist Figure 2 In FIG. 1 , an example is shown in which the current collector 11 is composed of a plurality of current collector particles, but the present invention is not limited to this case. Figure 3 This is an enlarged view of a characteristic portion of another example of the all-solid-state battery according to the first embodiment. Figure 3 The positive electrode current collector layer 1C shown is composed of a current collector 11. The current collector 11 may be in the form of a foil extending in the xy plane, a punched product, or an expanded product.

[0058] The positive electrode includes a positive electrode active material layer in contact with at least one main surface of the current collector layer. The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may also contain a conductive additive, a binder, and a solid electrolyte described below.

[0059] The thickness of the positive electrode active material layer can be set within a range of 1 μm to 500 μm.

[0060] [Positive electrode active material layer]

[0061] The positive electrode active material layer 1B is formed on one or both sides of the positive electrode collector layer 1A. The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may also contain a conductive additive, a binder, and the above-mentioned solid electrolyte. When the positive electrode active material layer 1B contains a solid electrolyte, the area between the uppermost xy plane passing through the positive electrode active material and the xy plane passing through the lowermost part is regarded as the positive electrode active material layer 1B.

[0062] (Positive electrode active material)

[0063] The positive electrode active material is not particularly limited as long as it can reversibly release and adsorb lithium ions, and detach and insert lithium ions. For example, a positive electrode active material used in a known lithium ion secondary battery can be used.

[0064] The positive electrode active material is, for example, a composite transition metal oxide, a transition metal fluoride, a polyanion, a transition metal sulfide, a transition metal oxyfluoride, a transition metal oxysulfide, and a transition metal oxynitride. The positive electrode active material is preferably a lithium manganese composite oxide, a lithium nickel composite oxide, a lithium cobalt composite oxide, a lithium vanadium composite oxide, a lithium titanium composite oxide, manganese dioxide, titanium oxide, niobium oxide, vanadium oxide, tungsten oxide, etc. For example, the positive electrode active material is LiCoO2, LiMnO2, preferably LiCoO2. These compounds may also deviate from the stoichiometric composition.

[0065] For example, the positive electrode active material may be Li x Lithium cobalt oxide represented by CoO2 is a material in which x changes in the range of 0.4 to 1.2 as the all-solid-state battery is charged and discharged.

[0066] In addition, as the positive electrode active material, a positive electrode active material that does not contain lithium can also be used. These positive electrode active materials are prepared by pre-arranging a negative electrode active material doped with metallic lithium or lithium ions at the negative electrode, and the battery can be used from the start of discharge. For example, lithium-free metal oxides (MnO2, V2O5, etc.), lithium-free metal sulfides (MoS2, etc.), lithium-free fluorides (FeF3, VF3, etc.), etc. are examples of these positive electrode active materials.

[0067] (Conductive additive)

[0068] The conductive aid is not particularly limited as long as it improves the electron conductivity in the positive electrode active material layer 1B, and a known conductive aid can be used. The conductive aid may include, for example, carbon materials such as graphite, carbon black, graphene, and carbon nanotubes, or metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO, or mixtures thereof. The conductive aid may also be in the form of powder or fiber.

[0069] (Bonding material)

[0070] The binder bonds the positive electrode current collector layer 1A and the positive electrode active material layer 1B, the positive electrode active material layer 1B and the solid electrolyte layer 3 , and various materials constituting the positive electrode active material layer 1B.

[0071] The binder can be used within the range that does not eliminate the function of the positive electrode active material layer 1B. The binder may not be contained if it is not necessary. The content of the binder in the positive electrode active material layer 1B is, for example, 0.5 to 30% by volume of the positive electrode active material layer. When the content of the binder is sufficiently small, the resistance of the positive electrode active material layer 1B becomes sufficiently low.

[0072] As long as the bonding material can be joined as described above, for example, fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) can be cited. In addition, in addition to the above, as bonding materials, for example, cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, polyamide-imide resin, etc. can also be used. In addition, as bonding materials, conductive polymers with electronic conductivity and ion conductive polymers with ion conductive properties can also be used. As conductive polymers with electronic conductivity, for example, polyacetylene can be cited. In this case, the bonding material also plays the role of a conductive auxiliary agent, so it is also possible not to add a conductive auxiliary agent. As ion conductive polymers with ion conductive properties, for example, substances that conduct lithium ions can be used, such as monomers of polymer compounds (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazenes, etc.) and lithium salts such as LiClO4, LiBF4, LiPF6 or alkali metal salts with lithium as the main body are compounded to obtain substances, etc. The polymerization initiator used for composite formation may be, for example, a photopolymerization initiator or a thermal polymerization initiator suitable for the above-mentioned monomers. The properties required of the adhesive material include oxidation and reduction resistance and good adhesiveness.

[0073] So far, specific examples of positive electrodes have been shown, but the positive electrodes are not limited to these examples. Figure 4 and Figure 5 This is a cross-sectional view of another example of the positive electrode according to the first embodiment.

[0074] Figure 4 The positive electrode shown has a positive electrode collector layer 1D and a positive electrode active material layer 1B. The positive electrode collector layer 1D has a collector 11, a positive electrode active material 12, and an oxide 13. The oxide 13 is, for example, an oxide containing Ag, such as AgCoO2. The oxide 13 prevents oxidation of Ag contained in the collector 11. When the oxide 13 is present between the collector 11 and the positive electrode active material 12, the cycle characteristics of the all-solid-state battery 10 are improved.

[0075] Figure 5 The positive electrode shown has a positive electrode current collector layer 1E, an intermediate layer 1F, and a positive electrode active material layer 1B. The positive electrode current collector layer 1E has a current collector 11 and an oxide 13. The intermediate layer 1F is composed of the oxide 13. Figure 5 The example shown corresponds to a thickness of oxide 13 of Figure 4The example shown is thick. The oxide 13 prevents oxidation of Ag contained in the current collector 11, and the cycle characteristics of the all-solid battery 10 are improved.

[0076] "Solid electrolyte layer"

[0077] The solid electrolyte layer 3 includes a solid electrolyte. The solid electrolyte is a substance that can move ions by an electric field applied from the outside. For example, the solid electrolyte layer 3 conducts lithium ions and blocks the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.

[0078] The solid electrolyte layer 3 includes a first solid electrolyte having a γ-Li3PO4 type crystal structure. The first solid electrolyte is, for example, Li 3+x Si x P 1-x O4、Li 3+x Si x V 1-x O4、Li 3+x Ge x P 1-x O4、Li 3+x Ge x V 1-x O4, etc. x satisfies 0.2≤x≤0.8. x may also satisfy 0.2≤x≤0.6. In addition, the first solid electrolyte may be a ternary lithium oxide containing Si, V, and Ge, etc.

[0079] "negative electrode"

[0080] The negative electrode 2 includes, for example, a current collector 21 and a second solid electrolyte 22. In this case, the area between the uppermost xy plane passing through the current collector 21 and the lowermost xy plane passing through the current collector 21 is regarded as the negative electrode 2. In addition, the negative electrode 2 may include a conductive additive, a binder, and the like.

[0081] The current collector 21 is composed of one or more selected from Ag and an alloy containing Ag. The alloy containing Ag is, for example, an AgPd alloy or an AgLi alloy. When the current collector 21 is an alloy containing Ag, the volume ratio of Ag contained in the alloy is, for example, 80% or more. Figure 3 As shown, the current collector 21 may be a foil extending in the xy plane, or may be in the form of a pressed product or a rolled product.

[0082] Ag and alloys containing Ag are compounds that can adsorb and release ions. Ag and alloys containing Ag show the function of a collector that conducts electrons toward the terminal electrodes 5 and 6, and the function of a negative electrode active material that performs charge and discharge. Therefore, the negative electrode 2 may not contain composite transition metal oxides, transition metal fluorides, polyanions, transition metal sulfides, transition metal oxyfluorides, transition metal oxysulfides, transition metal oxynitrides, etc. that usually act as negative electrode active materials. When Ag and alloys containing Ag with low potential act as negative electrodes 2, the output voltage from the all-solid-state battery 10 becomes large.

[0083] The negative electrode 2 may contain only Ag and Ag in an alloy containing Ag. The negative electrode 2 may contain only Ag and Ag in an alloy containing Ag. The negative electrode 2 may contain both Ag and Ag in an alloy containing Ag.

[0084] As the alloy containing Ag, for example, an Ag—Pd alloy or an Ag—Li alloy can be used.

[0085] The volume ratio (first volume ratio) of Ag or Ag alloy to the entire negative electrode 2 may be 45% to 95%, 50% to 90%, 60% to 80%, or 80% or more.

[0086] The second solid electrolyte 22 is the same as the first solid electrolyte contained in the above-mentioned solid electrolyte layer 3. The volume ratio (second volume ratio) of the second solid electrolyte 22 contained in the negative electrode 2 is, for example, 5% or more. The volume ratio of the second solid electrolyte 22 contained in the negative electrode 2 may be 5% or more and 55% or more, 10% or more and 50% or less, or 20% or more and 40% or less.

[0087] The first solid electrolyte and the second solid electrolyte 22 may have the same constituent elements.

[0088] The sum of the first volume ratio and the second volume ratio may be 95% or more and 100% or less.

[0089] In the negative electrode 2, the current collector 21 is in direct contact with the second solid electrolyte 22. The contact ratio between the current collector 21 and the second solid electrolyte 22 is, for example, 50% or more, preferably 80% or more. The contact ratio between the current collector 21 and the second solid electrolyte 22 is obtained by extracting any 10 points of the current collector 21 from a cross-sectional image measured by a scanning electron microscope, and dividing the length of the contact portion between the current collector 21 and the second solid electrolyte 22 by the outer circumference of the current collector 21.

[0090] "Method for manufacturing all-solid-state batteries"

[0091] Next, a method for manufacturing the all-solid-state battery 10 is described. First, the stacked body 4 is produced. The stacked body 4 is produced, for example, by a simultaneous firing method or a sequential firing method.

[0092] The simultaneous firing method is a method of manufacturing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of firing each layer after it is formed. The simultaneous firing method can manufacture the laminate 4 with fewer operation steps than the sequential firing method. In addition, the laminate 4 manufactured by the simultaneous firing method is denser than the laminate 4 manufactured by the sequential firing method. The following is an example of the case where the simultaneous firing method is used.

[0093] First, the materials constituting the positive electrode current collector layer 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, and the negative electrode 2 of the stacked body 4 are made into pastes. Figure 4 In the example shown, the current collector 11 is coated with the oxide 13 and then made into a paste. Figure 5 In the case of the example shown, the material constituting the intermediate layer 1F is also in the form of a paste.

[0094] The method of making each material into a paste is not particularly limited, and for example, a method of mixing powders of each material into a vehicle to obtain a paste can be used. Here, the vehicle is a general term for a medium in a liquid phase. The vehicle includes a solvent or a binder.

[0095] Next, a green sheet is prepared. The green sheet is obtained by applying the paste prepared according to each material on a substrate such as a PET (polyethylene terephthalate) film, drying it as needed, and then peeling off the substrate. The method for applying the paste is not particularly limited, and for example, a known method such as screen printing, coating, transfer, or scraping can be used.

[0096] Next, the green sheets made from each material are stacked in the desired order and number of layers to make a laminated sheet. When stacking the green sheets, alignment and cutting are performed as needed. For example, when making a parallel type or a series-parallel type battery, the green sheets are stacked while being aligned so that the end face of the positive electrode collector layer 1A and the end face of the negative electrode 2 do not coincide.

[0097] The laminated sheet can also be made by making a positive electrode unit and a negative electrode unit and stacking these units. The positive electrode unit is a laminated sheet obtained by stacking the solid electrolyte layer 3, the positive electrode active material layer 1B, the positive electrode collector layer 1A, and the positive electrode active material layer 1B in sequence. Figure 5In the example shown, an intermediate layer 1F is stacked between the positive electrode current collector layer 1A and the positive electrode active material layer 1B. The negative electrode unit is a laminated sheet obtained by sequentially stacking a solid electrolyte layer 3 and a negative electrode 2. The solid electrolyte layer 3 of the positive electrode unit and the negative electrode 2 of the negative electrode unit are stacked face to face, or the positive electrode active material layer 1B of the positive electrode unit and the solid electrolyte layer 3 of the negative electrode unit are stacked face to face.

[0098] Next, the produced laminated sheets are pressurized together to improve the adhesion of each layer. Pressing can be performed by, for example, a molding machine, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during crimping is, for example, set to 40 to 95° C. Next, the pressurized laminate is cut using a cutting device to form chips. Then, the chips are debonded and sintered to obtain a laminate 4 consisting of a sintered body.

[0099] The debinding process can be performed as a process different from the firing process. When the debinding process is performed, the binder component contained in the chip is heated and decomposed before the firing process, which can inhibit the rapid decomposition of the binder component in the firing process. The debinding process is performed by heating at a temperature of 300 to 800°C for 0.1 to 10 hours, for example, in an atmospheric atmosphere. The atmosphere of the debinding process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode and the solid electrolyte are not oxidized or reduced or are difficult to oxidize and reduce, and the gas type can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode and the solid electrolyte do not react with the atmospheric gas. For example, it can be performed in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere mixed with them.

[0100] The sintering process is carried out, for example, by placing the chip on a ceramic table. Firing is carried out, for example, by heating to 600 to 1000° C. in an atmospheric atmosphere. The sintering time is, for example, set to 0.1 to 3 hours. The atmosphere of the sintering process is an oxygen partial pressure environment in which the materials constituting the positive electrode, the negative electrode, and the solid electrolyte are not oxidized or reduced or are difficult to oxidize and reduce, and the type of gas can be arbitrarily selected so that the materials constituting the positive electrode, the negative electrode, and the solid electrolyte do not react with the atmospheric gas. For example, it can also be carried out in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, and an atmosphere mixed with them.

[0101] In addition, the sintered laminated body 4 (sintered body) can also be placed in a cylindrical container together with abrasive materials such as aluminum oxide and drum-ground. Thus, the chamfering of the corners of the laminated body can be performed. Grinding can also be performed using sandblasting. Sandblasting can only eliminate specific parts, so it is preferred.

[0102] Terminal electrodes 5 and 6 are formed on the mutually opposite sides of the manufactured stacked body 4. The terminal electrodes 5 and 6 can be formed by sputtering, impregnation coating, screen printing, spraying, etc. By going through the above steps, a solid-state battery 10 can be manufactured. When the terminal electrodes 5 and 6 are formed only in a predetermined portion, the above treatment is performed by covering with a tape or the like.

[0103] The energy density of the all-solid-state battery of this embodiment is high. This is considered to be because the potential of the negative electrode 2 becomes about 0 V (vs Li) due to the Ag and the alloy containing Ag in the negative electrode 2 acting as the negative electrode active material. + / Li). The all-solid-state battery 10 is connected to the negative electrode 2 with a potential of about 0V and a potential of about 3.6V (vs Li + / Li) is driven by the potential difference between the positive electrode 1 (LiCoO2 or LiMn2O4) of the all-solid-state battery, thereby increasing the output voltage of the all-solid-state battery. The energy of the all-solid-state battery 10 is obtained by the product of the output voltage of the all-solid-state battery 10 and the capacity of the all-solid-state battery. If the volumes of the all-solid-state batteries are the same, the energy density of the all-solid-state battery 10 can be compared in terms of energy. Therefore, the energy density of the all-solid-state battery of this embodiment is high.

[0104] In addition, when the negative electrode 2 comprises lithium titanium oxide (potential is about 1.5 V (vs Li + / Li)) etc., the above output voltage may not be achieved. The reason is not clear, but it is considered that the lithium titanium oxide preferentially accepts lithium ions due to the combination of structures that function as a negative electrode active material.

[0105] Although the embodiments of the present invention have been described in detail with reference to the drawings, each structure in each embodiment and their combination are merely examples, and addition, omission, replacement, and other changes to the structure may be made without departing from the spirit of the present invention.

[0106] Example

[0107] "Example 1"

[0108] (Production of positive electrode paste)

[0109] To prepare the positive electrode current collector layer paste, Ag, Pd, and LiMn2O4 were mixed in a volume ratio of 64:16:20. Ethyl cellulose and dihydroterpineol were added to the powder and mixed. Ethyl cellulose was a binder and dihydroterpineol was a solvent.

[0110] The positive electrode active material layer paste is prepared by adding ethyl cellulose and dihydroterpineol to LiMn2O4 and mixing the mixture.

[0111] (Preparation of Solid Electrolyte Layer Paste)

[0112] Li2CO3, SiO2, and Li3PO4 were used as the starting materials and mixed at a molar ratio of 2:1:1. Water was used as the dispersion medium during the mixing process and the mixture was wet-mixed in a ball mill for 16 hours. The mixed product was calcined at 950°C for 2 hours to produce Li 3.5 Si 0.5 P 0.5 Then, 100 parts by mass of the calcined powder, 100 parts by mass of ethanol, and 200 parts by mass of toluene were added to a ball mill for wet mixing. Then, 16 parts of a polyvinyl butyral binder and 4.8 parts by mass of butyl benzyl phthalate were further added and mixed to prepare a solid electrolyte layer paste.

[0113] (Preparation of negative electrode paste)

[0114] The negative electrode paste uses Ag, Pd, and Li 3.5 Si 0.5 P 0.5 O4 was mixed in a volume ratio of 76:19:5 to obtain a powder. Ethyl cellulose and dihydroterpineol were added to the powder and mixed.

[0115] (Fabrication of all-solid-state batteries)

[0116] Next, the positive electrode unit and the negative electrode unit were made in the following order. First, on the above-mentioned solid electrolyte layer sheet, the positive electrode active material layer paste was printed with a thickness of 5μm using screen printing. Then, the printed positive electrode active material layer paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode active material layer paste, the positive electrode collector layer paste was printed with a thickness of 5μm using screen printing. Next, the printed positive electrode collector layer paste was dried at 80°C for 5 minutes. Then, on the dried positive electrode collector layer paste, the positive electrode active material layer paste was printed again with a thickness of 5μm using screen printing and dried. Then, the PET film was peeled off. In this way, a positive electrode unit in which the positive electrode active material layer / positive electrode collector layer / positive electrode active material layer were stacked in sequence on the main surface of the solid electrolyte layer was obtained.

[0117] Next, the negative electrode paste was printed on the main surface of the solid electrolyte layer to a thickness of 10 μm. Next, the printed negative electrode paste was dried at 80° C. for 5 minutes.

[0118] As for the laminate, a solid electrolyte unit with 5 solid electrolyte layer sheets stacked on top of each other was produced. 50 electrode units (25 positive electrode units and 25 negative electrode units) were stacked alternately in a manner of sandwiching solid electrolyte units. At this time, the units were staggered and stacked in such a way that the odd-numbered electrode units only extended from one end face, and the even-numbered electrode units only extended from the end face on the opposite side. Six solid electrolyte layer sheets were stacked on the stacked unit. Then, they were formed and cut by hot pressing to produce a laminated chip. Then, the laminated chips were fired simultaneously to obtain a laminate. During simultaneous firing, the temperature was raised to a firing temperature of 800°C at a heating rate of 200°C / hour in an atmospheric atmosphere, maintained at this temperature for 2 hours, and naturally cooled after firing.

[0119] The terminal electrodes 5 and 6 are mounted on the sintered laminate (sintered body) by a known method to produce a solid-state battery. Figure 2 The volume ratio of each layer does not change between the paste state before sintering and the state after sintering. Ag has a form in which Ag exists as a single substance and a form in which Ag is contained as a contained element of an AgPd alloy.

[0120] Then, the output voltage and capacity of the fabricated all-solid-state battery were measured. The capacity is the discharge capacity. Under a 60°C environment, constant current charging (CC charging) was performed at a constant current of 100 μA until the battery voltage reached 3.9V. Then, the battery voltage was discharged (CC discharge) at a constant current of 100 μA until the battery voltage reached 0V. The above cycle was repeated for 10 cycles, and the discharge capacity (μAh) of the 10th cycle was measured. Then, the energy (μWh) was obtained from the product of the output voltage and capacity of the all-solid-state battery.

[0121] "Examples 2 to 5"

[0122] In Examples 2 to 5, the Li 3.5 Si 0.5 P 0.5 The amount of O4 added and the Li 3.5 Si 0.5 P 0.5 The other conditions were the same as those in Example 1, and the same measurements as in Example 1 were performed.

[0123] "Examples 6 to 10"

[0124] In Examples 6 to 10, the solid electrolyte used in preparing the solid electrolyte layer paste was changed to Li 3.5 Si 0.5 V 0.5 O4, and change the solid electrolyte added to the negative electrode paste to Li 3.5Si 0.5 V 0.5 O4, these two points are different from those of Examples 1 to 5. Other conditions are the same as those of Examples 1 to 5, and the same measurements as those of Examples 1 to 5 were performed.

[0125] "Example 11"

[0126] In Example 11, in the preparation of the positive electrode current collector layer paste, a powder obtained by mixing Ag, Pd, and LiCoO2 in a volume ratio of 64:16:20 was used, and the positive electrode active material layer paste was changed to LiMn2O4 and LiCoO2 was used, which are different from Example 2. Other conditions were the same as in Example 2, and the same measurements as in Example 2 were performed.

[0127] "Examples 12 to 15"

[0128] In Examples 12 to 15, the composition ratio of the solid electrolyte used in preparing the solid electrolyte layer paste was changed, which is different from Example 13. In Example 12, the solid electrolyte was Li 3.6 Si 0.6 P 0.4 O4, in Example 13, the solid electrolyte is set to Li 3.4 Si 0.4 P 0.6 O4, in Example 14, the solid electrolyte is set to Li 3.2 Si 0.2 P 0.8 O4, in Example 15, the solid electrolyte is Li 3.1 Si 0.1 P 0.9 The other conditions were the same as those in Example 11, and the same measurements as in Example 11 were performed.

[0129] "Example 16"

[0130] In Example 16, Ag and Li were used to prepare the negative electrode paste. 3.5 Si 0.5 P 0.5 The two points that the powder obtained by mixing Ag and LiCoO2 in a volume ratio of 80:20 was used to prepare the positive electrode paste are different from Example 11. The other conditions are the same as those in Example 11, and the same measurements as in Example 11 were performed.

[0131] "Examples 17 to 23"

[0132] In Examples 17 to 21), the Li 3.5 Si0.5 P 0.5 The amount of O4 added and the Li 3.5 Si 0.5 P 0.5 The other conditions were the same as those in Example 11, and the same measurements as in Example 11 were performed.

[0133] "Example 24"

[0134] In Example 24, the composition of the solid electrolyte used in preparing the negative electrode paste was changed to Li 3.4 Si 0.4 P 0.6 O4, which is different from Example 13.

[0135] "Example 25"

[0136] In Example 25, the solid electrolyte used in preparing the solid electrolyte paste was changed to Li 3.3 Si 0.3 P 0.7 O4, which is different from Example 29.

[0137] "Example 26"

[0138] In Example 26, the composition of the solid electrolyte used in preparing the negative electrode paste was changed to Li 3.6 Si 0.6 P 0.4 O4, which is different from Example 12.

[0139] "Examples 27 to 30"

[0140] In Examples 27 to 30, the composition ratio of the solid electrolyte used in preparing the negative electrode paste was changed, which is different from Example 11. In Example 27, the solid electrolyte was Li 3.4 Si 0.4 P 0.6 O4, in Example 28, the solid electrolyte is set to Li 3.6 Si 0.6 P 0.4 O4, in Example 29, the solid electrolyte is set to Li 3.3 Si 0.3 P 0.7 O4, in Example 30, the solid electrolyte is set to Li 3.2 Si 0.2 P 0.8 The other conditions were the same as those in Example 11, and the same measurements as in Example 11 were performed.

[0141] "Example 31"

[0142] In Example 31, the solid electrolyte used in preparing the negative electrode paste was changed to Li 3.5 Si 0.5 V 0.5 O4 is different from Example 11. Other conditions are the same as those of Example 11, and the same measurements as those of Example 11 are performed.

[0143] In Examples 32 and 33, Li-Ag alloy was added to the negative electrode collector layer and the same study was performed. However, the treatment of the Li-Ag alloy was carried out in a glove box with a dew point of -50°C, and during the sintering, the temperature was raised to 800°C at a heating rate of 1200°C / hour in an argon atmosphere, and the temperature was maintained for 20 minutes, and then naturally cooled after sintering.

[0144] "Examples 32-33"

[0145] In Example 32, when preparing the negative electrode current collector layer, part of Ag was replaced with Li-Ag alloy (Li 3.1 Ag) is different from Example 15. The Li content of the Li-Ag alloy is determined by quantitative analysis by X-ray diffraction (XRD). The other conditions are the same as those of Example 1.

[0146] In Example 33, when preparing the negative electrode current collector layer, part of Ag was replaced with Li-Ag alloy (Li 4.7 Ag) is different from Example 15. The Li content of the Li-Ag alloy is determined by quantitative analysis by X-ray diffraction (XRD). The other conditions are the same as those of Example 1.

[0147] "Comparative Example 1"

[0148] In Comparative Example 1, no Li was added when preparing the negative electrode paste. 3.5 Si 0.5 P 0.5 O4 was used, which was different from Example 1. The volume ratio of Ag to Pd was set to 80:20. Other conditions were the same as those in Example 1, and the same measurements as in Example 1 were performed.

[0149] "Comparative Example 2"

[0150] In Comparative Example 2, no Li was added when preparing the negative electrode paste. 3.5 Si 0.5 V 0.5 O4 was used, which was different from Example 6. The volume ratio of Ag to Pd was set to 80:20. Other conditions were the same as those in Example 6, and the same measurements as in Example 6 were performed.

[0151] "Comparative Example 3"

[0152] In Comparative Example 3, the negative electrode is set to a structure consisting of a negative electrode collector layer and a negative electrode active material layer, and its negative electrode unit is set to a unit obtained by stacking negative electrode active material layer / negative electrode collector layer / negative electrode active material layer in sequence on the main surface of the solid electrolyte layer. In the negative electrode collector layer, when making the paste, Ag and Pd were mixed in a volume ratio of 80:20 to prepare an AgPd alloy. The negative electrode active material layer paste was set to Li4Ti5O 12 (Li 4 / 3Ti 5 / 3 The other conditions were the same as those in Example 1, and the same measurements as in Example 1 were performed.

[0153] "Comparative Example 4"

[0154] In Comparative Example 4, when preparing the negative electrode paste, Li 3.5 Si 0.5 P 0.5 O4 and Li4Ti5O 12 (Li 4 / 3 Ti 5 / 3O4), which is different from Example 2. In making the negative electrode paste, Ag, Pd, and Li 4 / 3 Ti 5 / 3 O4 was mixed at a volume ratio of 64:16:20. Other conditions were the same as in Example 1, and the same measurements as in Example 1 were performed.

[0155] "Comparative Example 5"

[0156] Comparative Example 5 is different from Example 2 in that the composition ratio of the solid electrolyte used in preparing the solid electrolyte layer paste is changed. 3.1 Si 0.1 P 0.9 O4. The solid electrolyte has a crystal structure of Li4SiO4 type rather than a crystal structure of γ-Li3PO4 type. Other conditions were the same as those in Example 1, and the same measurements as in Example 1 were performed.

[0157] "Comparative Example 6"

[0158] In Comparative Example 6, the solid electrolyte layer is Li4Ti5O 12 , which is different from Example 16, is not the first solid electrolyte having a γ-Li3PO4 type crystal structure.

[0159] "Comparative Example 7"

[0160] In Comparative Example 7, the solid electrolyte contained in the negative electrode is Li4Ti5O 12 , which is different from Example 16, is not a second solid electrolyte having a γ-Li3PO4 type crystal structure.

[0161] "Comparative Example 8"

[0162] In Comparative Example 8, the negative electrode is set to a structure consisting of a negative electrode collector layer and a negative electrode active material layer, and its negative electrode unit is set to a unit obtained by stacking negative electrode active material layer / negative electrode collector layer / negative electrode active material layer in sequence on the main surface of the solid electrolyte layer. In the negative electrode collector layer, when making a paste, a powder obtained by mixing Ag and Pd in ​​a volume ratio of 80:20 was used to prepare an AgPd alloy. The negative electrode active material layer paste was set to Li4Ti5O 12 (Li 4 / 3Ti 5 / 3 The other conditions were the same as those in Example 16, and the same measurements as in Example 16 were performed.

[0163] The results of Examples 1 to 33 and Comparative Examples 1 to 8 are summarized in Tables 1 to 3 below.

[0164]

[0165]

[0166]

[0167] The energy of outputs of Examples 1 to 33 is greater than that of Comparative Examples 1 to 5. Since samples of the same size were prepared for Examples 1 to 33 and Comparative Examples 1 to 8, the energy density of outputs of Examples 1 to 33 is higher than that of Comparative Examples 1 to 8.

[0168] In Comparative Examples 1 and 2, the AgPd alloy functions as a negative electrode active material, and therefore the output voltage is large. On the other hand, in Comparative Examples 1 and 2, the contact area between the solid electrolyte and the AgPd alloy is limited, and sufficient capacity cannot be obtained. As a result, it is considered that Comparative Examples 1 and 2 cannot obtain sufficient energy compared with Examples 1 to 14.

[0169] In Comparative Examples 3 and 4, Li 4 / 3 Ti 5 / 3 O4 is contained in the negative electrode, so Li 4 / 3 Ti 5 / 3 O4 acts prior to the AgPd alloy, and a sufficient output voltage cannot be obtained. As a result, it is considered that compared with Examples 1 to 14, Comparative Examples 3 and 4 cannot obtain sufficient energy.

[0170] In Comparative Example 5, the solid electrolyte layer is a Li4SiO4 type crystal structure, not a γ-Li3PO4 type crystal structure. Compared with the γ-Li3PO4 type crystal structure, the Li4SiO4 type crystal structure has poor ion conductivity and cannot transmit sufficient lithium ions to the negative electrode, and it is believed that sufficient capacity cannot be obtained. As a result, it is believed that compared with Examples 1 to 14, Comparative Example 5 cannot obtain sufficient energy.

[0171] In Comparative Examples 6 to 8, it is believed that the capacity and energy are significantly reduced because any one of the following three points is not satisfied: the solid electrolyte layer has a first solid electrolyte having a γ-Li3PO4 type crystal structure, the negative electrode has a second solid electrolyte having a γ-Li3PO4 type crystal structure, and the negative electrode has one or more selected from Ag and an alloy containing Ag.

[0172] Industrial Applicability

[0173] Able to provide all-solid-state batteries with higher energy density than ever before.

Claims

1. An all-solid-state battery, wherein: A sintered body is provided, the sintered body having: a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode, The solid electrolyte layer has a first solid electrolyte having a γ-Li3PO4 type crystal structure, The negative electrode has a second solid electrolyte and one or more selected from Ag and an alloy containing Ag, and the second solid electrolyte has a γ-Li3PO4 type crystal structure.

2. The all-solid-state battery according to claim 1, wherein: The volume ratio of the second solid electrolyte to the entire negative electrode is 5% to 55%.

3. The all-solid-state battery according to any one of claims 1 to 3, wherein The first solid electrolyte comprises Li 3+x Si x P 1-x O4, where 0.2≤x≤0.

6.

4. The all-solid-state battery according to claim 1, wherein: The second solid electrolyte comprises Li 3+x Si x P 1-x O4, where 0.2≤x≤0.

6.

5. The all-solid-state battery according to claim 1, wherein: The first solid electrolyte and the second solid electrolyte have the same constituent elements.

6. The all-solid-state battery according to claim 1, wherein: The total volume ratio of the Ag and the alloy containing Ag to the entire negative electrode is 45% to 95%.

7. The all-solid-state battery according to claim 1, wherein: The sum of the volume ratio of the solid electrolyte to the entire negative electrode and the volume ratio of the Ag or the alloy containing Ag to the entire negative electrode is 95% or more and 100% or less.

8. The all-solid-state battery according to claim 1, wherein: The alloy containing Ag is a Li—Ag alloy.

9. The all-solid-state battery according to claim 1 or 2, wherein: The positive electrode includes lithium cobalt oxide.