All-solid-state secondary battery

By using Li3+xSixP1-xO4 as the main phase and a solid electrolyte layer containing boron-containing compounds containing lithium, boron, and oxygen as the secondary phase in an all-solid secondary battery, the problems of insufficient capacitance and high-temperature sintering reactions are solved, and a more efficient High capacitance and reliability.

CN118749151APending Publication Date: 2024-10-08TDK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092072.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-09-30
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing all-solid secondary batteries have insufficient capacitance, and the oxide solid electrolyte easily reacts with the active material during high-temperature sintering to form a layer with low ion conductivity, which affects battery performance.

Method used

A solid electrolyte layer containing Li3+xSixP1-xO4 as the main phase and a boron-containing compound containing lithium, boron, and oxygen as the secondary phase is used. The secondary phase is connected to the interface portion of the negative electrode layer and the solid electrolyte layer to form an all-solid state with large capacitance. Secondary battery.

Benefits of technology

By optimizing the chemical composition and distribution of the solid electrolyte layer, the capacitance of the battery is increased, the active material reaction during high-temperature sintering is avoided, and the reliability and capacitive performance of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118749151A_ABST
    Figure CN118749151A_ABST
Patent Text Reader

Abstract

An all-solid-state secondary battery is provided with a sintered body having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer, and is characterized in that the solid electrolyte layer contains: a main phase comprising an electrolyte represented by formula (1); and a sub-phase comprising a boron-containing compound containing lithium, boron, and oxygen. At least a portion of the sub-phase is in contact with a portion of an interface between the negative electrode layer and the solid electrolyte layer. Li3 + xSixP1-xO4 (1) (Formula (1) satisfies 0 < x < 1). )
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an all-solid secondary battery.

[0002] This application claims priority based on Tokugan Application No. 2022-058652 filed in Japan on March 31, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In recent years, the rapid development of electronic technology has achieved the miniaturization, lightness, thinness and multifunctionality of portable electronic devices. Along with this, for batteries that become the power source of electronic devices, it is strongly desired to be miniaturized, light-weighted, thinned and reliable. Therefore, all-solid secondary batteries using solid electrolytes as electrolytes have attracted much attention. At present, as solid electrolytes for all-solid secondary batteries, sulfide solid electrolytes and oxide solid electrolytes are mainly used.

[0004] Sulfide solid electrolytes have excellent plasticity, so by pressing powder, an interface between the solid electrolyte and the active material can be formed. However, sulfide solid electrolytes have safety issues because they produce hydrogen sulfide when reacting with water.

[0005] On the other hand, oxide solid electrolytes do not produce hydrogen sulfide due to reaction with water, so they are safe. However, in order to obtain high ion conductivity, oxide solid electrolytes need to be densified, so they need to be sintered at high temperatures. However, in the sintering process for forming a dense solid electrolyte layer, the oxide solid electrolyte reacts with the active material, and sometimes a reaction layer with low ion conductivity is generated at the interface between the oxide solid electrolyte and the active material.

[0006] LSPO (Li2PO4) is known as an oxide solid electrolyte that is relatively stable with respect to the active material even when sintered at high temperature for densification. 3+x Si x P 1-x O4) (see Non-Patent Document 1). However, LSPO has an ion conductivity as low as 1×10 -6 S / cm platform (see Non-Patent Document 2).

[0007] As a technique for improving the ion conductivity of LSPO, a method of adding boron as a sintering aid is known. For example, Non-Patent Document 1 describes that sintering is promoted by adding lithium borate to LSPO, thereby improving the ion conductivity.

[0008] In addition, as a lithium ion secondary battery having low internal resistance and high capacitance, Patent Document 1 describes an all-solid lithium ion secondary battery containing a compound composed of lithium and boron in a positive electrode layer, a negative electrode layer, and a solid electrolyte layer.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent No. 6455807 (B)

[0012] Non-patent literature

[0013] Non-patent document 1: Solid State Ionics 283 (2015) 109-114

[0014] Non-patent document 2: Ionics 7 (2001) 469-473 Summary of the invention

[0015] Problems to be solved by the invention

[0016] Currently, all-solid-state secondary batteries are required to further increase their capacitance.

[0017] The present invention has been developed in view of the above-mentioned problems, and its object is to provide an all-solid secondary battery with a large capacity.

[0018] Technical solutions to solve problems

[0019] In order to solve the above problems, the following technical solutions are provided.

[0020] [1] An all-solid secondary battery, characterized in that it comprises a sintered body having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer, the solid electrolyte layer comprising: a main phase composed of an electrolyte represented by the following formula (1); and a subphase composed of a boron-containing compound containing lithium, boron and oxygen, at least a portion of the subphase being in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer.

[0021] Li 3+x Si x P 1-x O4(1)

[0022] (Equation (1) satisfies 0<x<1.)

[0023] [2] The all-solid secondary battery according to [1], wherein the volume ratio of the subphase in the solid electrolyte layer is 1 volume % to 10 volume %.

[0024] [3] The all-solid secondary battery according to [1] or [2], wherein the subphase is formed of particles having a particle size of 0.1 μm to 3 μm.

[0025] [4] An all-solid secondary battery according to [1], wherein the proportion of the secondary phase existing in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer is greater than the proportion of the secondary phase existing in contact with a portion of the interface between the positive electrode layer and the solid electrolyte layer.

[0026] [5] The all-solid secondary battery according to [1], wherein the sum of the volume of the main phase and the volume of the sub-phase in the solid electrolyte layer is 90% by volume or more.

[0027] [6] The all-solid secondary battery according to any one of [1] to [3], wherein the negative electrode layer contains any one metal selected from the group consisting of Ag, Pd, Au and Pt.

[0028] Effects of the Invention

[0029] The all-solid secondary battery of the present invention has a solid electrolyte layer, which includes: a main phase (first phase) containing an electrolyte represented by formula (1); and a secondary phase (second phase) composed of a boron-containing compound containing lithium, boron and oxygen, and the secondary phase exists in a manner of contacting a portion of the interface between the negative electrode layer and the solid electrolyte layer. In the all-solid secondary battery of the present invention, the secondary phase in the solid electrolyte layer becomes the starting point of the reaction in the transfer of ions, and therefore, the capacitance is large. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic cross-sectional view showing an example of the all-solid secondary battery of the present invention.

[0031] Figure 2 Yes Figure 1 The schematic cross-sectional view showing an enlarged portion of the all-solid secondary battery 10 is shown.

[0032] Figure 3 It is a schematic cross-sectional view showing another example of the all-solid secondary battery of the present invention. DETAILED DESCRIPTION

[0033] In order to solve the above-mentioned problems and to provide an all-solid secondary battery with a large capacity, the present inventors have repeatedly conducted intensive studies focusing on the solid electrolyte layer as shown below.

[0034] First, the present inventors studied the case of using an electrolyte represented by the following formula (1) and a boron-containing compound as materials for a solid electrolyte layer.

[0035] Li 3+x Si x P 1-x O4(1)

[0036] (Equation (1) satisfies 0<x<1.)

[0037] Non-patent document 1 describes an all-solid lithium-ion secondary battery, in which an electrolyte represented by formula (1), a lithium compound Li2CO3, and a boron compound H3BO4 are used as materials for a solid electrolyte layer. However, the technology described in non-patent document 1 does not provide an all-solid secondary battery with a sufficiently large capacity.

[0038] Therefore, the present inventors further conducted studies focusing on the chemical composition and distribution of the boron-containing compound contained in the solid electrolyte layer.

[0039] As a result, it was found that the solid electrolyte layer can be made as follows, that is, the solid electrolyte layer comprises: a main phase containing an electrolyte represented by formula (1); and a subphase composed of a boron-containing compound containing lithium, boron and oxygen, and the subphase exists in a manner that is in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer, thereby completing the present invention.

[0040] In an all-solid secondary battery having such a solid electrolyte layer, the secondary phase that is in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer becomes the starting point of the reaction in the transfer of lithium ions. As a result, it is estimated that the all-solid secondary battery has a large capacity.

[0041] In addition, there is no record in non-patent document 1 about an all-solid-state secondary battery manufactured using boron-containing compounds containing lithium, boron and oxygen, such as lithium borate, as a material for a solid electrolyte layer, and its capacitance. At present, the capacitance improvement effect in an all-solid-state secondary battery using boron-containing compounds containing lithium, boron and oxygen as a material for a solid electrolyte layer has not been confirmed.

[0042] Hereinafter, the all-solid secondary battery of the present embodiment will be described in detail with reference to the accompanying drawings as appropriate. In the drawings used in the following description, in order to facilitate the understanding of the features of the present invention, the features are sometimes enlarged for convenience. Therefore, the size ratios of the various components are sometimes different from the actual ones. The materials, dimensions, etc. exemplified in the following description are only examples, and the present invention is not limited to these, and can be appropriately changed and implemented within the scope of not changing its purpose.

[0043] [All-solid-state secondary battery]

[0044] Figure 1 It is a schematic cross-sectional view showing an example of the all-solid secondary battery of the present invention. Figure 2 Yes Figure 1 The schematic cross-sectional view showing an enlarged portion of an all-solid secondary battery is shown.

[0045] exist Figure 1 In the figure, reference numeral 10 denotes an all-solid secondary battery according to the present embodiment. Figure 1The all-solid secondary battery 10 shown has a stack 4, a first external terminal 5, and a second external terminal 6. The first external terminal 5 and the second external terminal 6 are formed of a conductive material. The first external terminal 5 and the second external terminal 6 are respectively connected to the opposite surfaces of the stack 4. The first external terminal 5 and the second external terminal 6 extend in a direction intersecting (orthogonal) with the stacking surface of the stack 4.

[0046] The laminate 4 includes a positive electrode layer 1, a negative electrode layer 2, and a solid electrolyte layer 3 sandwiched between the positive electrode layer 1 and the negative electrode layer 2. The laminate 4 is a sintered body formed by laminating the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3 and sintering them. The number of layers of the positive electrode layer 1 and the negative electrode layer 2 contained in the laminate 4 may be one layer each, or two or more layers each. Figure 1 As shown, the solid electrolyte layer 3 is not only between the positive electrode layer 1 and the negative electrode layer 2, but also between the positive electrode layer 1 and the second external terminal 6, and between the negative electrode layer 2 and the first external terminal 5. Figure 1 As shown, one end of the positive electrode layer 1 is connected to the first external terminal 5 , and one end of the negative electrode layer 2 is connected to the second external terminal 6 .

[0047] The all-solid secondary battery 10 is charged or discharged by transferring ions between the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3. Figure 1 A laminated all-solid secondary battery 10 is shown.

[0048] [Solid electrolyte layer]

[0049] The solid electrolyte layer 3 can move ions by an externally applied electric field. The solid electrolyte layer 3 conducts lithium ions, for example, and blocks the movement of electrons. The solid electrolyte layer 3 includes: a main phase containing a solid electrolyte represented by the following formula (1); and a subphase composed of a boron-containing compound containing lithium, boron, and oxygen.

[0050] Li 3+x Si x P 1-x O4(1)

[0051] (Equation (1) satisfies 0<x<1.)

[0052] The main phase contains a solid electrolyte represented by formula (1). The solid electrolyte represented by formula (1) is a compound that is relatively stable relative to the active material even when sintered at a high temperature for densification. Therefore, the all-solid-state battery 10 of the present embodiment is not easy to deteriorate and has excellent reliability. The solid electrolyte represented by formula (1) only needs to satisfy 0<x<1 to become a solid electrolyte that is further stable relative to the active material, and therefore, it is more preferable to satisfy 0.3≤x≤0.8. The solid electrolyte represented by formula (1) that forms the main phase may be only one type or two or more solid electrolytes with different x in formula (1), and can be determined appropriately according to the necessary characteristics required by the all-solid-state battery 10.

[0053] The main phase may also be composed only of the solid electrolyte represented by formula (1). In the main phase, compounds other than the electrolyte represented by formula (1) may also be included within the range that does not impair the effect of the present invention. As compounds other than the electrolyte represented by formula (1), for example, known compounds used as solid electrolytes may be cited. Specifically, it may also be a compound in which a portion of P in formula (1) is substituted by at least one element selected from Ti, Co, Mn, and Ni.

[0054] The main phase may contain, for example, a compound and / or an element derived from a sintering aid, an active material forming the positive electrode layer 1 and / or the negative electrode layer 2 , or the like.

[0055] The subphase is composed of a boron-containing compound containing lithium, boron and oxygen. The boron-containing compound forming the subphase can be any compound containing lithium, boron and oxygen, or it can be a compound containing not only lithium, boron and oxygen, but also elements such as phosphorus and carbon. The above-mentioned boron-containing compound is preferably a sintered body, or it can be, for example, Li3BO3, LiBO2, B4Li2O7, LiBPO4, etc. The above-mentioned boron-containing compound can also be a glass containing lithium, boron, phosphorus and oxygen. In order to become a fully solid secondary battery 10 with a larger capacitance, the boron-containing compound forming the subphase is particularly preferably Li3BO3. The above-mentioned boron-containing compound forming the subphase can be only one kind, or it can be more than two kinds, which can be determined appropriately according to the necessary characteristics required by the fully solid secondary battery 10.

[0056] In this embodiment, for manufacturing reasons such as improving productivity and yield when forming the solid electrolyte layer 3, a sintering aid may be used in combination with the electrolyte represented by formula (1) and a compound that is a boron-containing compound containing lithium, boron and oxygen as the material of the solid electrolyte layer 3. In this case, the main phase of the solid electrolyte layer 3 may also contain a compound (the compound is not a compound containing lithium, boron and oxygen) and / or an element that is not removed and remains in the firing process for manufacturing the stack 4. In addition, in this case, the subphase may also include: a boron-containing compound containing lithium, boron and oxygen; and a compound (the compound is not a compound containing lithium, boron and oxygen) and / or an element that is not removed and remains in the firing process for manufacturing the stack 4.

[0057] As the sintering aid, any known sintering aid can be used as long as it has a sinterability improving effect. Specifically, as the sintering aid, for example, compounds containing zinc (Zn), bismuth (Bi), etc. can be mentioned.

[0058] like Figure 2 As shown, the solid electrolyte layer 3 in the all-solid secondary battery 10 of the present embodiment is composed of a main phase 31 formed in a layered manner over the entire region between the positive electrode layer 1 and the negative electrode layer 2 , and a plurality of particulate subphases 32 .

[0059] In the solid electrolyte layer 3 in the all-solid secondary battery 10 of the present embodiment, the subphase 32 exists in contact with a portion of the interface between the negative electrode layer 2 and the solid electrolyte layer 3. As a result, the all-solid secondary battery 10 of the present embodiment has a larger capacitance than, for example, an all-solid secondary battery in which the subphase exists on the entire surface of the interface with the negative electrode layer 2 in the solid electrolyte layer 3, and an all-solid secondary battery in which the subphase exists approximately uniformly throughout the entire solid electrolyte layer 3.

[0060] The reason why the all-solid secondary battery has a large capacity is not yet determined, but it is estimated that, for example, the subphase 32 in the solid electrolyte layer 3 functions as a starting point for a reaction in lithium ion transfer.

[0061] In the all-solid secondary battery 10 of the present embodiment, all of the subphases 32 contained in the solid electrolyte layer 3 are preferably present in contact with the interface between the negative electrode layer 2 and the solid electrolyte layer 3. In this case, all of the subphases 32 act as starting points for reactions in the transfer of lithium ions in the solid electrolyte layer 3, thereby achieving an all-solid secondary battery 10 with a greater capacity. In the all-solid secondary battery 10 of the present embodiment, there may be a subphase 32 that is not in contact with the interface between the negative electrode layer 2 and the solid electrolyte layer 3 within the range in which the effects of the present invention are obtained.

[0062] The subphase 32 may also be composed of a plurality of particles (blocks). A portion of the clusters of these plurality of particles may also be in contact with the interface between the solid electrolyte layer 3 and the positive electrode layer 1. In this case, the proportion (volume proportion) of the subphase particles in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer among the plurality of particles may also be greater than the proportion of the subphase particles in contact with a portion of the interface between the positive electrode layer and the solid electrolyte layer among the plurality of particles.

[0063] The ratio of the proportion (volume proportion) of the subphase particles contained in the solid electrolyte layer that are in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer, and the ratio (volume proportion) of the subphase particles contained in the solid electrolyte layer that are in contact with a portion of the interface between the positive electrode layer and the solid electrolyte layer, can be greater than 1 or greater than 1.5.

[0064] In addition, in the solid electrolyte layer 3 in the all-solid secondary battery 10 of the present embodiment, the main phase 31 is formed in layers in the entire region between the positive electrode layer 1 and the negative electrode layer 2, and therefore, the sub-phase 32 is not in contact with the positive electrode layer 1. As a result, the sub-phase 32 functions more effectively as a starting point for the reaction in the transfer of lithium ions in the solid electrolyte layer 3, resulting in an all-solid secondary battery 10 with a larger capacity.

[0065] The shape and size of the subphase 32 contained in the solid electrolyte layer 3 are not particularly limited. For example, it may be in the form of a thin sheet or a thick sheet. Figure 2 The granular form is shown. Figure 2 As shown, when a plurality of subphases 32 exist in the solid electrolyte layer 3 , the shapes and sizes of the plurality of subphases 32 may be substantially uniform or non-uniform.

[0066] like Figure 2 As shown, when a plurality of granular subphases 32 are dispersed along the interface between the solid electrolyte 3 and the negative electrode layer 2, the subphase 32 acts more effectively as a starting point for the reaction in the transfer of lithium ions in the solid electrolyte layer 3, thereby achieving a fully solid secondary battery 10 with a larger capacity.

[0067] The subphase 32 present in the solid electrolyte 3 is preferably a particle with an average particle size of 0.1μm to 3μm, and more preferably a particle with an average particle size of 0.1μm to 1μm. In the case where the subphase 32 is a particle with an average particle size of 0.1μm to 3μm, the specific surface area of ​​the subphase 32 is sufficiently large. Therefore, the subphase 32 acts more effectively as the starting point of the reaction in the transfer of lithium ions. Moreover, in the case where the subphase 32 is a particle with an average particle size of 0.1μm to 3μm, the ion conduction of the main phase 31 is not easily hindered by the subphase 32. For these reasons, in the case where the subphase 32 is a particle with an average particle size of 0.1μm to 3μm, it becomes an all-solid secondary battery 10 with a further greater capacity.

[0068] The volume ratio of the subphase 32 contained in the solid electrolyte layer 3 is preferably 1 volume % or more and 10 volume % or less, more preferably 1 volume % or more and 5 volume % or less, and further preferably 1 volume % or more and 3 volume % or less. When the volume ratio of the subphase 32 is 1 volume % or more, the subphase 32 is fully present in the solid electrolyte layer 3, so the subphase 32 acts more effectively as the starting point of the reaction in the transfer of lithium ions. Therefore, it becomes a fully solid secondary battery 10 with a larger capacity. In addition, when the volume ratio of the subphase 32 is 1 volume % or more, the subphase 32 formed by sintering and combining the compound containing lithium, boron and oxygen, which is a boron-containing compound, is easy to become a particle with a particle size of 0.1 μm or more, so it is preferred. In addition, when the volume ratio of the subphase 32 is 10 volume % or less, the compound containing lithium, boron and oxygen, which is a boron-containing compound, is sintered and combined, and it is easy to form a subphase 32 divided in the surface direction. As a result, a plurality of particulate subphases 32 are dispersed along the interface between the solid electrolyte 3 and the negative electrode layer 2, and a solid electrolyte layer 3 in which the main phase 31 is arranged between adjacent subphases 32 and between the subphase 32 and the positive electrode active material layer 1B is easily formed, resulting in a fully solid secondary battery 10 with a larger capacity. In addition, when the volume ratio of the subphase 32 is 10% by volume or less, the subphase 32 formed by sintering and combining a boron-containing compound containing lithium, boron and oxygen is easy to become particles with a particle size of 3 μm or less, so it is preferred.

[0069] The sum of the volume of the main phase 31 and the volume of the subphase 32 in the solid electrolyte layer 3 may be 90% by volume or more, or 100% by volume or less.

[0070] [Positive electrode layer]

[0071] like Figure 1 As shown, the positive electrode layer 1 includes, for example, a positive electrode current collector 1A and a positive electrode active material layer 1B. Figure 1 As shown, the positive electrode active material layer 1B may be formed on both surfaces of the positive electrode current collector 1A, or may be formed on only one surface.

[0072] (Positive electrode collector)

[0073] The positive electrode current collector 1A has high electrical conductivity. The positive electrode current collector 1A includes, for example, a metal such as silver, palladium, gold, platinum, aluminum, copper, nickel, stainless steel, iron, and an alloy thereof, a conductive resin, and other conductive materials. The positive electrode current collector 1A may also include, for example, a positive electrode active material such as lithium cobalt oxide (LiCoO2), a lithium vanadium compound (LiV2O5, Li3V2(PO4)3, LiVOPO4), and the like.

[0074] (Positive Electrode Active Material Layer)

[0075] The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive auxiliary agent and a solid electrolyte.

[0076] (Positive electrode active material)

[0077] The positive electrode active material is not particularly limited as long as it can reversibly release and absorb lithium ions, and remove and insert lithium ions. For example, a positive electrode active material used in a known lithium ion secondary battery can be used.

[0078] The positive electrode active material is preferably one or two or more selected from, for example, composite transition metal oxides and transition metal composite oxides.

[0079] Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and lithium nickel oxide (LiNiO2). x Co y Mn z M a O2 (x+y+z+a=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤a≤1, M represents one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr) represented by a composite metal oxide, lithium titanate (Li4Ti5O 12 )wait.

[0080] As the positive electrode active material, a positive electrode active material that does not contain lithium can also be used. For the positive electrode active material that does not contain lithium, it can be used in the following manner: a negative electrode active material doped with metallic lithium and / or lithium ions is pre-configured in the negative electrode layer 2, and the all-solid secondary battery 10 is operated from discharge. As the positive electrode active material that does not contain lithium, for example, metal oxides (MnO2, V2O5, etc.) can be cited.

[0081] (Conductive additive)

[0082] The conductive aid is not particularly limited as long as it is a material that improves the electron conductivity in the positive electrode active material layer 1B, and a known conductive aid can be used. The conductive aid includes carbon materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO (indium tin oxide), or mixtures thereof. The conductive aid may also be in the form of powder or fiber.

[0083] (Solid Electrolyte)

[0084] The solid electrolyte contained in the positive electrode active material layer 1B makes the ion conductivity in the positive electrode active material layer 1B good. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. As the solid electrolyte, the same compound as the compound forming the above-mentioned solid electrolyte layer 3 can also be included.

[0085] [Negative electrode layer]

[0086] Figure 1 The negative electrode layer 2 shown serves as both a negative electrode current collector and a negative electrode active material layer. The negative electrode layer 2 exhibits a lower potential than the positive electrode active material. The negative electrode layer 2 preferably contains any metal selected from silver (Ag), palladium (Pd), gold (Au) and platinum (Pt). This is because Ag, Pd, Au and Pt do not melt and are not easily oxidized even when the sintering process for making the stack 4 is carried out in an atmospheric atmosphere. The negative electrode layer 2 can be composed of any of the above metals, and can also be composed of an alloy containing any of the above metals.

[0087] The negative electrode layer 2 particularly preferably contains an AgPd alloy. This is because the subphase 32 contained in the solid electrolyte layer 3 that is in contact with the negative electrode layer 2 acts more effectively as the starting point of the reaction in the transfer of lithium ions, thereby further increasing the capacitance. In addition, when the negative electrode layer 2 contains an AgPd alloy, it will become an all-solid secondary battery 10 with high energy density, so it is preferred. As an AgPd alloy, for example, an alloy containing Ag and Pd in ​​a molar ratio of 8:2 (Ag:Pd) can be used.

[0088] The negative electrode layer 2 may include: metal particles composed of any of the above metals and / or alloy particles composed of an alloy containing any of the above metals; and at least one selected from a conductive additive and a solid electrolyte.

[0089] (Conductive additive)

[0090] The conductive auxiliary agent improves the electron conductivity of the negative electrode layer 2. As the conductive auxiliary agent, the same material as that of the positive electrode active material layer 1B can be used.

[0091] (Solid Electrolyte)

[0092] The solid electrolyte contained in the negative electrode layer 2 makes the ion conduction in the negative electrode layer 2 good. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. As the solid electrolyte, the same compound as the compound forming the above-mentioned solid electrolyte layer 3 can also be included.

[0093] [Method for manufacturing all-solid-state secondary battery]

[0094] Next, a method for manufacturing the all-solid secondary battery 10 of the present embodiment will be described.

[0095] First, the laminate 4 is produced. The laminate 4 can be produced, for example, by a simultaneous firing method or a sequential firing method, preferably by a simultaneous firing method. The simultaneous firing method is a method of producing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of firing each layer each time it is formed. The simultaneous firing method can produce the laminate 4 by fewer operating steps than the sequential firing method. In addition, the laminate 4 produced by the simultaneous firing method is denser than the laminate 4 produced by the sequential firing method. Hereinafter, the method for producing the laminate 4 by the simultaneous firing method will be described as an example.

[0096] First, the materials constituting the positive electrode current collector 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3 and the negative electrode layer 2 of the laminate 4 are paste-formed to prepare a paste corresponding to the material of each layer.

[0097] In this embodiment, as pastes for solid electrolyte layer 3, a first paste containing an electrolyte represented by formula (1) and a second paste containing a compound that is a boron-containing compound containing lithium, boron and oxygen are prepared. The first paste is used to form main phase 31. The second paste is used to form subphase 32.

[0098] The first paste is obtained, for example, by paste-forming particles composed of an electrolyte represented by formula (1) and, if necessary, a sintering aid. The particles composed of an electrolyte represented by formula (1) can be produced by a known production method.

[0099] The second paste is obtained by, for example, pasting particles of a boron-containing compound containing lithium, boron and oxygen and, if necessary, a sintering aid. The second paste may further contain particles composed of an electrolyte represented by formula (1) as necessary.

[0100] As the particles of boron-containing compounds containing lithium, boron and oxygen used as the material of the second paste, for example, particles with an average particle size of 0.01 μm to 10 μm can be used, and particles with an average particle size of 0.1 μm to 3 μm are preferably used. When the above-mentioned average particle size is greater than 0.01 μm, when the particles of boron-containing compounds containing lithium, boron and oxygen are paste-formed, the particles of boron-containing compounds containing lithium, boron and oxygen are not easy to agglomerate in the paste, so it is preferred. When the above-mentioned average particle size is less than 10 μm, the average particle size is sufficiently small, and it is easy to generate multiple subphases 32 with a large specific surface area. As a result, the role of the subphase 32 as the starting point of the reaction of the donation and acceptance of lithium ions is more effectively obtained. The above-mentioned average particle size can be appropriately determined according to the composition of the subphase 32, the particle size, the heating temperature in the sintering process, and the sintering time.

[0101] There is no particular limitation on the method of paste-forming each material for manufacturing the laminate 4. For example, a method of obtaining a paste by mixing the powder of each material in a carrier can be adopted. Here, carrier is a general term for a medium in a liquid phase. The carrier of the present embodiment includes a solvent, a bonding material (adhesive), and a plasticizer. As a solvent, for example, dihydroterpineol can be used. As an adhesive, for example, ethyl cellulose can be used.

[0102] Next, a green sheet is prepared. The green sheet is obtained by applying the paste prepared according to the respective materials on a substrate such as a PET (polyethylene terephthalate) film, drying as required, and then peeling off the substrate. There is no particular limitation on the method for applying the paste, and for example, a known method such as screen printing, coating, transfer, and a doctor blade method can be used.

[0103] Next, the green sheets made of the respective materials are stacked in the desired order and stacking number to produce a laminated sheet. When stacking the green sheets, alignment and cutting are performed as required. For example, in the case of manufacturing a parallel type or a series-parallel type battery, it is preferred to stack the green sheets by aligning them so that the end face of the positive electrode collector 1A and the end face of the negative electrode collector 2A do not coincide.

[0104] The green sheets to be the laminated sheets may be the solid electrolyte layer unit, the positive electrode unit, and the green sheets to be the negative electrode layer 2 that have been fabricated in advance.

[0105] As the production order of the positive electrode unit, first, the paste for the positive electrode active material layer 1B is printed on a substrate such as a PET film by screen printing and dried to form the positive electrode active material layer 1B. Next, the paste for the positive electrode collector 1A is printed on the positive electrode active material 1B by screen printing and dried to form the positive electrode collector 1A. Next, the paste for the positive electrode active material layer 1B is printed on the positive electrode collector 1A by screen printing and dried to form the positive electrode active material layer 1B. Then, the positive electrode unit is obtained by peeling off the PET film. The positive electrode unit is a raw sheet in which the positive electrode active material layer 1B, the positive electrode collector 1A and the positive electrode active material layer 1B are stacked in sequence.

[0106] In addition, regarding the solid electrolyte layer unit, the first paste is applied to a substrate such as a PET film by a doctor blade method and dried to form a sheet. Next, the second paste is applied to the sheet made using the first paste by a doctor blade method and dried to form a sheet. The solid electrolyte layer unit is a raw sheet in which a sheet made using the first paste and a sheet made using the second paste are stacked.

[0107] Next, the produced positive electrode unit and the green sheet to be the negative electrode layer 2 are stacked via the solid electrolyte layer unit. At this time, the sheet made using the second paste in the solid electrolyte layer unit is arranged and stacked in a face-to-face manner with the green sheet to be the negative electrode layer 2. Thus, a laminated sheet is obtained in which the positive electrode active material layer 1B, the positive electrode collector 1A, the positive electrode active material layer 1B, the sheet made using the first paste, the sheet made using the second paste, the green sheet to be the negative electrode layer 2, the sheet made using the second paste, and the sheet made using the first paste are stacked in this order.

[0108] In addition, when stacking the positive electrode unit, the solid electrolyte layer unit, and the raw sheet to become the negative electrode layer 2, they are stacked alternately in a staggered manner so that the positive electrode unit extends only to one end face of the stacked sheet, and the raw sheet to become the negative electrode layer 2 extends only to the end face on the opposite side of the stacked sheet.

[0109] Next, the prepared lamination sheets are pressed together to improve the adhesion of each layer to form a laminate. Pressing can be performed by, for example, a die press, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during pressurization can be, for example, 40 to 95°C.

[0110] Next, the laminated substrate obtained after the pressurization is cut using a dicing device to obtain laminated chips. The obtained laminated chips are then subjected to a binder removal and sintering step. Thus, a laminated body 4 consisting of a sintered body is obtained.

[0111] The debinding and firing process can be performed by placing the laminate on a ceramic table, for example. The debinding and firing process is, for example, a process of heating to 550° C. to 1100° C. in an air atmosphere. The heating time (firing time) can be, for example, 0.1 hour to 6 hours. The heating temperature and firing time in the debinding and firing process can be appropriately determined according to the composition of each layer constituting the laminate 4, etc.

[0112] In the present embodiment, by performing the debinding and sintering steps, the particles of the boron-containing compound containing lithium, boron and oxygen contained in the second paste are bonded to each other and thus integrated. As a result, the sheet made using the second paste (a coating film formed on the sheet made using the first paste) arranged face to face with the negative electrode layer 2 is reduced in the surface direction and broken, generating a granular subphase 32, and forming a main phase 31 between adjacent subphases 32. The boron-containing compound containing lithium, boron and oxygen that becomes the subphase 32 is not easy to solid dissolve with the electrolyte represented by formula (1) that becomes the main phase 31, and also acts as a sintering aid for the solid electrolyte layer 3. As a result, a plurality of granular subphases 32 are dispersed along the interface between the solid electrolyte 3 and the negative electrode layer 2, forming a solid electrolyte layer 3 in which the main phase 31 is arranged between adjacent subphases 32 and between the subphase 32 and the positive electrode active material layer 1B.

[0113] The heating temperature in the debinding and firing steps is preferably 550°C to 1100°C, and more preferably 600°C to 1000°C. When the heating temperature in the debinding and firing steps is 550°C or higher, the bonding of the particles of the boron-containing compound containing lithium, boron and oxygen contained in the second paste is promoted. As a result, the sheet made using the second paste arranged face to face with the negative electrode layer 2 is easily reduced in the surface direction and broken. As a result, a plurality of granular subphases 32 are dispersed along the interface between the solid electrolyte 3 and the negative electrode layer 2, and a solid electrolyte layer 3 in which the main phase 31 is arranged between adjacent subphases 32 and between the subphase 32 and the positive electrode active material layer 1B is easily formed. In addition, when the heating temperature in the firing step is 1100°C or lower, it is possible to prevent the boron-containing compound containing lithium, boron and oxygen that becomes the subphase 32 and the electrolyte represented by formula (1) that becomes the main phase 31 from becoming a solid solution.

[0114] The sintered laminate 4 (sintered body) can also be placed in a cylindrical container together with a grinding material such as aluminum oxide, and ground by a drum grinding method. Thus, the chamfering of the corners of the laminate 4 can be performed. The grinding of the laminate 4 can also be performed by sandblasting. Sandblasting can only reduce specific parts of the surface of the laminate 4, so it is preferred.

[0115] Next, first external terminals 5 and second external terminals 6 are formed on mutually opposing side surfaces of the produced laminated body 4. The first external terminals 5 and second external terminals 6 can be formed by sputtering, dipping, screen printing, spraying, or the like.

[0116] By going through the above steps, the all-solid secondary battery 10 can be manufactured.

[0117] In the present embodiment, in the method for manufacturing the all-solid secondary battery 10, any one or more of the following conditions (1) to (7) are appropriately changed to obtain the all-solid secondary battery 10 having the solid electrolyte layer 3 in which the volume ratio of the subphase 32 and the particle size of the subphase 32 are within the desired range.

[0118] (1) Composition of particles of a boron-containing compound containing lithium, boron, and oxygen contained in the second paste.

[0119] (2) Average particle size of particles of the boron-containing compound containing lithium, boron, and oxygen contained in the second paste.

[0120] (3) When the second paste contains particles composed of an electrolyte represented by formula (1), the composition of the particles composed of the electrolyte represented by formula (1).

[0121] (4) When the second paste contains particles composed of an electrolyte represented by formula (1), the ratio of the particles composed of an electrolyte represented by formula (1) to the particles of a boron-containing compound containing lithium, boron and oxygen contained in the second paste.

[0122] (5) The ratio of the thickness of the sheet produced using the first paste to the thickness of the sheet produced using the second paste.

[0123] (6) Composition of particles composed of the electrolyte represented by formula (1) contained in the first paste.

[0124] (7) Heating temperature and firing time in the binder removal and firing steps.

[0125] In this embodiment, it is also possible to use: instead of the particles of the boron-containing compound containing lithium, boron and oxygen contained in the second paste, or while using the particles of the boron-containing compound containing lithium, boron and oxygen, one or more compounds that become boron-containing compounds containing lithium, boron and oxygen by firing and / or particles composed of one or more elements that become boron-containing compounds containing lithium, boron and oxygen by firing.

[0126] As the material for the second paste, the compound and / or element that becomes a boron-containing compound containing lithium, boron and oxygen, for example, boron oxide, boric acid, boron hydroxide, lithium borate, lithium oxide, lithium carbonate, lithium phosphate, etc. The particles (powder) of the compound that becomes these boron-containing compounds and / or the particles (powder) of the element that becomes these boron-containing compounds can be manufactured by a known manufacturing method, and one kind can be used or two or more kinds can be mixed and used according to the composition of the boron-containing compound containing lithium, boron and oxygen as the target.

[0127] As particles of compounds and / or elements that become boron-containing compounds containing lithium, boron and oxygen, for example, particles with an average particle size of 0.01 μm to 10 μm can be used, and particles with an average particle size of 0.1 μm to 3 μm are preferably used. When the above-mentioned average particle size is 0.01 μm or more, when the particles of the above-mentioned compounds and / or elements are paste-formed, the particles of the above-mentioned compounds and / or elements are not easy to agglomerate in the paste, so it is preferred. When the above-mentioned average particle size is 10 μm or less, the specific surface area of ​​the particles is sufficiently large, and thus, in the firing process, the reaction of generating boron-containing compounds containing lithium, boron and oxygen is well performed, so it is preferred. In addition, when the above-mentioned average particle size is 10 μm or less, the average particle size is sufficiently small, and it is easy to generate multiple subphases 32 with a large specific surface area. As a result, the function of the subphase 32 as the starting point of the reaction of lithium ion donation and acceptance is more effectively obtained. The above-mentioned average particle size can be appropriately determined according to the composition and particle size of the subphase 32 , the heating temperature and firing time in the firing step, and the like.

[0128] Figure 1 and Figure 2 The all-solid secondary battery 10 of the present embodiment shown has a sintered body, which has a positive electrode layer 1, a negative electrode layer 2, and a solid electrolyte layer 3 sandwiched between the positive electrode layer 1 and the negative electrode layer 2, and the solid electrolyte layer 3 includes: a main phase 31 containing an electrolyte represented by formula (1); and a subphase 32 composed of a boron-containing compound containing lithium, boron and oxygen. Moreover, the subphase 32 exists in a manner that is in contact with a portion of the interface between the negative electrode layer 2 and the solid electrolyte layer 3. Therefore, in the all-solid secondary battery 10 of the present embodiment, the subphase 32 in the solid electrolyte layer 3 becomes the starting point of the reaction in the transfer of lithium ions. As a result, a large-capacity all-solid secondary battery 10 is obtained.

[0129] Although the embodiments of the present invention have been described in detail with reference to the drawings, each structure in each embodiment and their combination are merely examples, and addition, omission, replacement, and other changes to the structure may be made without departing from the spirit of the present invention.

[0130] For example, in the all-solid secondary battery 10 of the above-mentioned embodiment, Figure 1As shown, the case where the negative electrode layer 2 serves as both the negative electrode collector and the negative electrode active material layer is illustrated as an example, but the negative electrode layer in the all-solid secondary battery of the present invention may also have a negative electrode collector and a negative electrode active material layer separately.

[0131] Figure 3 3 is a schematic cross-sectional view showing another example of the all-solid secondary battery of the present invention. Figure 1 The same components of the all-solid secondary battery 10 shown are denoted by the same reference numerals, and description thereof will be omitted. Figure 3 The all-solid secondary battery 20 shown is Figure 1 The illustrated all-solid secondary battery 10 differs only in the negative electrode layer 21 .

[0132] Figure 3 The negative electrode layer 21 in the all-solid secondary battery 20 shown in the figure has, for example, a negative electrode current collector 2A and a negative electrode active material layer 2B. The negative electrode active material layer 2B may be Figure 3 Although it is formed on both surfaces of the negative electrode current collector 2A as shown, it may be formed on only one surface.

[0133] (Negative electrode current collector)

[0134] The negative electrode current collector 2A is the same as the positive electrode current collector 1A. Specifically, for example, a material containing a metal such as silver, palladium, gold, platinum, aluminum, copper, nickel, stainless steel, iron, or alloys thereof, or a conductive material such as a conductive resin can be used as the negative electrode current collector 2A.

[0135] (Negative Electrode Active Material Layer)

[0136] The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may also contain a conductive additive and a solid electrolyte. As the conductive additive and the solid electrolyte that may be contained in the negative electrode active material layer 2B, the following can be used: Figure 1 The substance contained in the negative electrode layer 2 of the all-solid secondary battery 10 shown is the same substance.

[0137] (Negative electrode active material)

[0138] The negative electrode active material is a compound that can absorb and release ions. The negative electrode active material is a compound that exhibits a lower potential than the positive electrode active material. As the negative electrode active material, the same material as the positive electrode active material can be used. The negative electrode active material and the positive electrode active material used in the all-solid secondary battery 10 are determined in consideration of the potential of the negative electrode active material and the potential of the positive electrode active material.

[0139] Figure 3 The all-solid secondary battery 20 shown can be manufactured by, for example, the method shown below.

[0140] That is, the negative electrode unit shown below is used instead of the green sheet to be the negative electrode layer 2 produced in the above-mentioned embodiment, and in addition, Figure 1 and Figure 2 The all-solid secondary battery 10 is manufactured by the same method as the manufacturing method of the all-solid secondary battery 10 shown in FIG.

[0141] The negative electrode unit can be produced in the same order as the positive electrode unit produced in the above-mentioned embodiment. Specifically, first, a paste for the negative electrode active material layer 2B is printed on a substrate such as a PET film by screen printing and dried to form the negative electrode active material layer 2B. Next, a paste for the negative electrode collector 2A is printed on the negative electrode active material layer 2B by screen printing and dried to form the negative electrode collector 2A. Next, a paste for the negative electrode active material layer 2B is printed on the negative electrode collector 2A by screen printing and dried to form the negative electrode active material layer 2B. Then, the negative electrode unit is obtained by peeling off the PET film. The negative electrode unit is a raw sheet in which the negative electrode active material layer 2B, the negative electrode collector 2A, and the negative electrode active material layer 2B are stacked in sequence.

[0142] exist Figure 3 In the all-solid secondary battery 20 shown, Figure 1 and Figure 2 The all-solid secondary battery 10 shown in the figure also has a solid electrolyte layer 3, which includes: a main phase 31 containing an electrolyte represented by formula (1); and a subphase 32 composed of a boron-containing compound containing lithium, boron and oxygen, and the subphase 32 exists in a manner that is in contact with a portion of the interface between the negative electrode layer 2 and the solid electrolyte layer 3. Therefore, Figure 3 In the all-solid secondary battery 20 shown, Figure 1 and Figure 2 Similar to the all-solid secondary battery 10 shown, the subphase 32 in the solid electrolyte layer 3 also serves as a starting point for the reaction in the transfer of lithium ions, thereby achieving an all-solid secondary battery with a large capacity.

[0143] Example

[0144] Example 1

[0145] (Preparation of Solid Electrolyte Layer Paste)

[0146] As pastes for the solid electrolyte layer, a first paste and a second paste were produced by the following method.

[0147] (First Cream)

[0148] Will be by Li 3+x Si x P 1-xParticles composed of O4 (x in formula (1) is 0.5), ethyl cellulose, and dihydroterpineol were added to a ball mill and wet mixed to prepare a 15 volume % Li 3+x Si x P 1-x The first paste of Example 1 is composed of particles composed of O4 (x in the formula (1) is 0.5).

[0149] (Second ointment)

[0150] Particles composed of Li3BO3 (trilithium borate) with an average particle size of 0.5 μm, which are particles of a boron-containing compound containing lithium, boron and oxygen, ethyl cellulose, and dihydroterpineol are added to a ball mill for wet mixing to prepare a second paste of Example 1 containing 2 volume % of particles of a boron-containing compound containing lithium, boron and oxygen.

[0151] (Preparation of positive electrode collector paste)

[0152] A powder of an Ag-Pd alloy containing Ag and Pd at a molar ratio of 8:2 (Ag:Pd), ethyl cellulose, and dihydroterpineol were added to a ball mill and wet mixed to prepare a positive electrode current collector paste of Example 1.

[0153] (Preparation of positive electrode active material layer paste)

[0154] Lithium cobalt oxide (LiCoO 2 ), ethyl cellulose, and dihydroterpineol were added to a ball mill and wet mixed to prepare a positive electrode active material layer paste of Example 1 containing 15 volume % of lithium cobalt oxide (LiCoO 2 ) particles.

[0155] (Preparation of negative electrode layer paste)

[0156] A powder of an Ag-Pd alloy containing Ag and Pd at a molar ratio of 8:2 (Ag:Pd), ethyl cellulose, and dihydroterpineol were added to a ball mill and wet mixed to prepare a negative electrode layer paste of Example 1 containing 15 volume % of AgPd powder.

[0157] Ethyl cellulose used in each of the above-mentioned pastes is a binder and dihydroterpineol is a solvent.

[0158] (Fabrication of positive electrode unit)

[0159] On a substrate composed of a PET (polyethylene terephthalate) film, a positive electrode active material layer paste is applied with a thickness of 5 μm by screen printing and dried at 80°C for 5 minutes. On the dried positive electrode active material layer paste, a positive electrode collector paste is applied with a thickness of 5 μm by screen printing and dried at 80°C for 5 minutes. On the dried positive electrode collector paste, a positive electrode active material layer paste is applied with a thickness of 5 μm by screen printing, dried at 80°C for 5 minutes, and then peeled off from the substrate. Thus, a positive electrode unit having a positive electrode active material layer, a positive electrode collector, and a positive electrode active material layer stacked in sequence is obtained.

[0160] (Fabrication of Solid Electrolyte Layer Unit)

[0161] On a substrate composed of a PET (polyethylene terephthalate) film, the first paste was applied by screen printing at a thickness of 20 μm, and dried at 80°C for 10 minutes. On the dried first paste, the second paste was applied by screen printing at a thickness of 1 μm, dried at 80°C for 5 minutes, and then peeled from the substrate. Thus, a solid electrolyte layer unit in which a sheet made using the first paste and a sheet made using the second paste were stacked was obtained.

[0162] (Preparation of Green Sheet to Become Negative Electrode Layer)

[0163] The negative electrode layer paste was applied to a substrate made of a PET (polyethylene terephthalate) film by screen printing to a thickness of 5 μm, dried at 80° C. for 5 minutes, and then peeled from the substrate. In this way, a green sheet to be the negative electrode layer was obtained.

[0164] (Fabrication of all-solid-state secondary batteries)

[0165] Four positive electrode units and four green sheets that will become negative electrode layers are alternately stacked in a manner that sandwiches solid electrolyte layer units to obtain a laminated sheet that will become a laminated body 4. At this time, the sheets made using the second paste in the solid electrolyte layer unit in the laminated sheet are arranged face to face with the green sheets that will become negative electrode layers. In addition, the laminated sheets are stacked in a manner that the uppermost and lowermost surfaces of the laminated sheets become solid electrolyte layer units. In addition, the positive electrode units are extended only to one end face of the laminated sheet, and the green sheets that will become negative electrode layers are extended only to the end face on the opposite side, and the laminated sheets are stacked in a staggered manner.

[0166] Next, the laminated sheets were pressed together and cut using a cutting device to produce laminated chips. Then, the laminated chips were subjected to binder removal and sintering to obtain a laminated body of Example 1 consisting of a sintered body. When removing the binder, the laminated chips were heated at 500° C. for 10 hours in an atmospheric atmosphere, thereby performing a binder removal treatment on the laminated chips. The sintering was performed at 900° C. for 1 hour in an atmospheric atmosphere.

[0167] Next, the first external terminal and the second external terminal were formed on the mutually opposing side surfaces of the produced laminated body by Au sputtering.

[0168] Through the above process, we have Figure 1 An all-solid secondary battery 10 of Example 1 is shown.

[0169] Example 2

[0170] The all-solid secondary battery 10 of Example 2 was obtained in the same manner as Example 1 except that the volume ratio (volume %) of the boron-containing compound particles containing lithium, boron and oxygen in the second paste was set three times that of Example 1 to produce a solid electrolyte layer unit.

[0171] Example 3

[0172] The all-solid secondary battery 10 of Example 3 was obtained in the same manner as Example 1 except that the volume ratio (volume %) of the boron-containing compound particles containing lithium, boron and oxygen in the second paste was set 15 times that of Example 1 to produce a solid electrolyte layer unit.

[0173] Example 4

[0174] The all-solid secondary battery 10 of Example 4 was obtained in the same manner as Example 1 except that the volume ratio (volume %) of the boron-containing compound particles containing lithium, boron and oxygen in the second paste was set to 0.5 times that of Example 1 to produce a solid electrolyte layer unit.

[0175] Example 5

[0176] The all-solid secondary battery 10 of Example 5 was obtained in the same manner as in Example 1 except that particles composed of Li 3 BO 3 (trilithium borate) with an average particle size of 0.2 μm were used as particles of a boron-containing compound containing lithium, boron and oxygen to prepare the second paste.

[0177] Example 6

[0178] The second paste is prepared using particles composed of Li3BO3 (trilithium borate) with an average particle size of 5 μm as particles of a boron-containing compound containing lithium, boron and oxygen. The volume ratio (volume %) of the particles of the boron-containing compound containing lithium, boron and oxygen in the second paste is set to 0.1 times that of Example 1. The second paste is applied on the dried first paste with a thickness of 10 μm to prepare a solid electrolyte layer unit. Except for this, the same procedure as Example 1 is followed to obtain an all-solid secondary battery 10 of Example 6.

[0179] Example 7

[0180] The all-solid secondary battery 10 of Example 7 was obtained in the same manner as in Example 1 except that particles composed of Li 3 BO 3 (trilithium borate) with an average particle size of 0.05 μm were used as particles of a boron-containing compound containing lithium, boron and oxygen to prepare the second paste.

[0181] Example 8

[0182] The negative electrode layer is changed to Cu / lithium titanate (Li4Ti5O 12 ) and the firing atmosphere was changed to a nitrogen atmosphere, the same procedure as in Example 1 was followed to obtain an all-solid secondary battery 10 of Example 8. The negative electrode layer was formed in the following order.

[0183] First, lithium titanate powder, ethyl cellulose and dihydroterpineol were added to a ball mill for wet mixing to prepare a second negative electrode paste containing 15 volume % of lithium titanate particles. Next, Cu powder, ethyl cellulose and dihydroterpineol were added to a ball mill for wet mixing to prepare a negative electrode current collector paste containing 15 volume % of Cu particles.

[0184] Next, on a substrate composed of a PET (polyethylene terephthalate) film, a second negative electrode layer paste was applied with a thickness of 5 μm by screen printing, dried at 80° C. for 5 minutes, a negative electrode collector paste was applied, dried for 5 minutes, a second negative electrode layer paste was applied with a thickness of 5 μm, dried at 80° C. for 5 minutes, and then peeled from the substrate. Thus, a negative electrode layer having a second negative electrode layer / negative electrode collector layer / second negative electrode layer stacked in sequence was obtained.

[0185] Example 9

[0186] As the paste for the solid electrolyte layer, the first paste and the second paste of Example 1 were prepared by mixing Li 3+x Si x P 1-x A paste in which particles composed of O4 (x in formula (1) is 0.5) are mixed with particles of a boron-containing compound containing lithium, boron and oxygen in a volume ratio of 100:1 is used to replace the first paste. Except for this, the same procedure as in Example 1 is carried out to obtain an all-solid secondary battery 10 of Example 9.

[0187] Example 10

[0188] The all-solid secondary battery 10 of Example 10 was obtained in the same manner as in Example 1 except that the second paste was prepared using particles composed of Li 3 BO 3 (trilithium borate) having an average particle size of 1 μm as particles of a boron-containing compound containing lithium, boron and oxygen.

[0189] Embodiment 11

[0190] The all-solid secondary battery 10 of Example 11 was obtained in the same manner as in Example 6 except that the second paste was prepared using particles composed of Li 3 BO 3 (trilithium borate) having an average particle size of 3.0 μm as particles of a boron-containing compound containing lithium, boron and oxygen.

[0191] Example 12

[0192] The all-solid secondary battery 12 of Example 13 was obtained in the same manner as in Example 6 except that the second paste was prepared using particles composed of Li 3 BO 3 (trilithium borate) with an average particle size of 3.2 μm as particles of a boron-containing compound containing lithium, boron and oxygen.

[0193] Embodiment 13

[0194] The all-solid secondary battery 10 of Example 13 was obtained in the same manner as Example 1 except that the volume ratio (volume %) of the boron-containing compound particles containing lithium, boron and oxygen in the second paste was set to 10 times that of Example 1 to produce a solid electrolyte layer unit.

[0195] Embodiment 14

[0196] The all-solid secondary battery 10 of Example 14 was obtained in the same manner as Example 1 except that the volume ratio (volume %) of the boron-containing compound particles containing lithium, boron and oxygen in the second paste was set to 11 times that of Example 1 to produce a solid electrolyte layer unit.

[0197] Embodiment 15

[0198] A second paste was prepared in the same manner as in Example 1 except that particles composed of Li 3 BO 3 (trilithium borate) having an average particle size of 0.05 μm were used as particles of a boron-containing compound containing lithium, boron and oxygen.

[0199] Next, in the preparation of the solid electrolyte layer unit, the first paste is applied at a thickness of 10 μm by screen printing on a substrate composed of a PET (polyethylene terephthalate) film, and the paste is dried at 80°C for 10 minutes. On the dried first paste, the second paste is applied at a thickness of 1 μm by screen printing, and the paste is dried at 80°C for 5 minutes and then peeled off from the substrate, thereby preparing the first solid electrolyte layer unit.

[0200] Next, the first paste was applied at a thickness of 10 μm and dried at 80°C for 10 minutes. The second paste was applied at a thickness of 1.25 μm by screen printing on the dried first paste, dried at 80°C for 5 minutes, and then peeled off from the substrate to prepare the second solid electrolyte layer unit.

[0201] The first solid electrolyte layer unit and the second solid electrolyte layer unit are attached with the solid electrolyte layers facing each other, thereby obtaining a third solid electrolyte layer unit which is stacked in sequence with a sheet made using the second paste having a thickness of 1 μm, a sheet made using the first paste having a thickness of 20 μm, and a sheet made using the second paste having a thickness of 1.25 μm.

[0202] In addition, the all-solid secondary battery 10 of Example 15 was obtained in the same manner as Example 1, except that the third solid electrolyte unit was arranged so that the first solid electrolyte unit faced the raw sheet that would become the negative electrode layer, and the second solid electrolyte unit faced the raw sheet that would become the positive electrode layer.

[0203] Example 16

[0204] The all-solid secondary battery 10 of Example 16 was obtained in the same manner as in Example 15 except that the second paste of the second solid electrolyte layer unit had a thickness of 1 μm.

[0205] Embodiment 17

[0206] The all-solid secondary battery 10 of Example 17 was obtained in the same manner as in Example 15 except that the second paste of the second solid electrolyte layer unit had a thickness of 0.8 μm.

[0207] Embodiment 18

[0208] The all-solid secondary battery 10 of Example 18 was obtained in the same manner as in Example 15 except that the second paste of the second solid electrolyte layer unit had a thickness of 0.7 μm.

[0209] Comparative Example 1

[0210] An all-solid secondary battery 10 of Comparative Example 1 was obtained in the same manner as in Example 1 except that a stacking sheet to be a solid electrolyte layer produced by the method described below was used instead of the solid electrolyte layer unit.

[0211] The first paste of Example 1 was applied to a substrate composed of a PET (polyethylene terephthalate) film by screen printing at a thickness of 20 μm, dried at 80° C. for 10 minutes, and then peeled from the substrate. Thus, a laminating sheet serving as a solid electrolyte layer was obtained.

[0212] Comparative Example 2

[0213] An all-solid secondary battery 10 of Comparative Example 2 was obtained in the same manner as in Example 1 except that a green sheet to be a solid electrolyte layer produced by the method described below was used instead of the solid electrolyte layer unit.

[0214] The first paste and the second paste of Example 1 were made of Li3+x Si x P 1-x The solid electrolyte layer paste of Comparative Example 2 was prepared by mixing particles composed of O 4 (x in Formula (1) is 0.5) and particles of a boron-containing compound containing lithium, boron and oxygen at a volume ratio of 100:1.

[0215] The solid electrolyte layer paste was applied to a substrate made of PET (polyethylene terephthalate) film by screen printing to a thickness of 20 μm, dried at 80° C. for 10 minutes, and then peeled from the substrate. Thus, a green sheet to be a solid electrolyte layer of Comparative Example 2 was obtained.

[0216] Comparative Example 3

[0217] In addition to using Li 1.3 Al 0.3 Ti 1.7 An all-solid secondary battery 10 of Comparative Example 3 was obtained in the same manner as in Example 1 except that (PO 4 ) 3 was used as the solid electrolyte.

[0218] Tables 1 to 3 show the compositions of the negative electrode layers of the all-solid secondary batteries 10 of Examples 1 to 18 and Comparative Examples 1 to 3 obtained in this manner.

[0219]

[0220]

[0221]

[0222] In addition, for the all-solid secondary batteries 10 of Examples 1 to 18 and Comparative Examples 1 to 3, the location of the secondary phase, the volume ratio (volume %) of the secondary phase in the solid electrolyte layer, and the particle size (μm) of the secondary phase were determined by the following method. The results are shown in Tables 1 to 3.

[0223] The all-solid secondary battery 10 is cut to expose the cross section, and a polished cross section is obtained using a cross section polisher (CP). The all-solid secondary battery 10 is cut in a manner that separates the approximately central portion between the first external terminal and the second external terminal when the laminate is observed from the laminate surface. Then, the obtained cross section is observed at 5000 times using a scanning electron microscope (SEM) to obtain reflected electron images of 10 viewing fields.

[0224] Based on the contrast of the reflected electron images of the 10 viewing fields obtained, the main phase and the sub-phase in the positive electrode layer, the negative electrode layer, and the solid electrolyte layer were respectively identified.

[0225] Then, it is confirmed whether the subphase exists in the solid electrolyte layer. In addition, if the subphase exists in the solid electrolyte layer, it is checked whether the existence site is in contact with a part of the interface between the solid electrolyte layer and the negative electrode layer.

[0226] In addition, for the all-solid secondary battery 10 in which a subphase exists in the solid electrolyte layer, each reflected electron image is converted into a black and white image and binarized. Then, the number of pixels corresponding to the subphase in each field of view is measured and added up respectively. Next, the volume ratio of the subphase is calculated for each field of view by the formula shown below, and the average value of the 10 fields of view is set as the volume ratio (volume %) of the subphase.

[0227] Volume ratio of the secondary phase (volume %) = (number of pixels of the secondary phase in the field of view / total number of pixels in the field of view) × 100

[0228] In addition, in the all-solid secondary battery 10 in which a subphase exists in the solid electrolyte layer, for the reflected electron images of the above 10 fields of view, the subphases identified by contrast are extracted respectively, and the average value of each particle size is calculated and set as the particle size (μm) of the subphase. In the case where the cross-sectional shape of the subphase is not circular (amorphous in the cross-sectional view), the diameter of the long axis direction of the subphase is set as the particle size.

[0229] In addition, the initial capacitance (μA) of the all-solid secondary batteries 10 of Examples 1 to 18 and Comparative Examples 1 to 3 was determined by the following method. The results are shown in Tables 1 to 3.

[0230] (Measurement of initial capacitance (μA))

[0231] The capacitor is a discharge capacitor. In an environment of 60°C, constant current charging (CC charging) is performed at a constant current of 10μA until the battery voltage reaches 3.9V, and then, discharge (CC discharge) is performed at a constant current of 10μA until the battery voltage reaches 0V. The above process is set as one cycle, and the discharge capacitance (μAh) of the tenth cycle after repeating the process ten times is measured.

[0232] As shown in Tables 1 to 3, it was confirmed that the all-solid secondary battery 10 of Example 118 contained a subphase in the solid electrolyte layer, and the subphase existed in contact with a part of the interface between the negative electrode layer and the solid electrolyte layer.

[0233] In addition, the all-solid secondary batteries 10 of Examples 1 to 18 have a larger initial capacity than the all-solid secondary battery of Comparative Example 1 in which no secondary phase exists in the solid electrolyte layer, and the all-solid secondary battery of Comparative Example 2 in which the secondary phase exists substantially uniformly throughout the solid electrolyte layer. The reason for this is estimated to be that in the all-solid secondary batteries 10 of Examples 1 to 18, a secondary phase that serves as a starting point for a reaction in lithium ion transfer exists at the interface between the solid electrolyte layer and the negative electrode layer.

[0234] In particular, in Example 1, in which the volume ratio of the subphase in the solid electrolyte layer is 1 volume %, and in Example 2, in which the volume ratio of the subphase is 3 volume %, the initial capacitance is larger than that in Example 4, in which the volume ratio of the subphase is 0.5 volume %, and in Example 3, in which the volume ratio of the subphase is 15 volume %.

[0235] In Example 1, in which the particle size of the subphase in the solid electrolyte layer was 0.5 μm, the initial capacitance was larger than that of Example 5, in which the particle size of the subphase was 0.2 μm, and Example 7, in which the particle size of the subphase was 0.05 μm.

[0236] In Example 1, in which the particle size of the subphase in the solid electrolyte layer was 0.5 μm, the initial capacitance was larger than that of Example 6, in which the particle size of the subphase was 5 μm, and Example 10, in which the particle size of the subphase was 1 μm.

[0237] Industrial Applicability

[0238] It can provide all-solid-state batteries that are safer and have greater capacity than existing batteries.

[0239] Description of Reference Numerals

[0240] 1 positive electrode layer; 1A positive electrode current collector; 1B positive electrode active material layer;

[0241] 2, 21 negative electrode layer; 2A negative electrode current collector; 2B negative electrode active material layer;

[0242] 3 solid electrolyte layer; 4 laminate; 5 first external terminal;

[0243] 6 second external terminal; 10, 20 all-solid secondary battery; 31 main phase; 32 auxiliary phase.

Claims

1. An all-solid secondary battery, characterized in that: A sintered body is provided, the sintered body having: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer sandwiched between the positive electrode layer and the negative electrode layer, The solid electrolyte layer includes: a main phase composed of an electrolyte represented by the following formula (1); and a subphase composed of a boron-containing compound containing lithium, boron and oxygen, At least a portion of the subphase is in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer. Li 3+x Yes x P 1-x O4(1) Formula (1) satisfies 0<x<1.

2. The all-solid secondary battery according to claim 1, wherein: The volume ratio of the subphase in the solid electrolyte layer is 1 volume % to 10 volume %.

3. The all-solid secondary battery according to claim 1 or 2, wherein: The subphase is formed of particles having a particle size of 0.1 μm to 3 μm.

4. The all-solid secondary battery according to claim 1, wherein: The ratio of the subphase existing in contact with a portion of the interface between the negative electrode layer and the solid electrolyte layer is greater than the ratio of the subphase existing in contact with a portion of the interface between the positive electrode layer and the solid electrolyte layer.

5. The all-solid secondary battery according to claim 1, wherein: The sum of the volume of the main phase and the volume of the subphase in the solid electrolyte layer is 90 volume % or more.

6. The all-solid secondary battery according to any one of claims 1 to 3, wherein The negative electrode layer contains any one metal selected from Ag, Pd, Au and Pt.