Low temperature hydrothermal re-lithiation of spent lithium ion battery cathodes by redox mediation
Through the low-temperature hydrothermal relithiation process and the use of green additives, the safety hazards and energy consumption problems of high temperature and high pressure in lithium-ion battery cathode recycling are solved, safe and energy-saving low-temperature relithiation is achieved, and the NCM material is ensured. Effective recycling and electrochemical performance restoration.
Patent Information
- Application Number
- CN202380023478.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-24
- Filing Date
- 2023-02-23
- Publication Date
- 2024-10-08
AI Technical Summary
Existing lithium-ion battery cathode recycling methods have safety hazards and high energy consumption caused by high-temperature smelting processes, and the traditional hydrothermal relithiation process requires high temperatures and high pressures, making it difficult to perform safely and effectively in large-scale operations.
The low-temperature hydrothermal relithiation process (LTHR) is used to improve the relithiation kinetics of waste NCM materials through a low-concentration redox mediator (red redox mediator), reduce the relithiation temperature to 100°C or lower, and use Green additives such as ethanol, ethylene glycol and hydrogen peroxide reduce processing stress.
It achieves safe and efficient recycling of degraded NCM cathode materials under environmental pressure, reduces energy consumption and operating costs, significantly improves safety, and shows the same effectiveness as high-temperature processes on different NCM materials.
Smart Images

Figure CN118749155A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit of priority to U.S. Provisional Application No. 63 / 313,677, filed on February 24, 2022, which is incorporated herein by reference.
[0003] Government Rights
[0004] This invention was made with government support under Grant No. DE-AC02-06CH11357 (SUB 9F-60081) awarded by the Department of Energy and Grant No. CBET1805570 awarded by the National Science Foundation. The Government has certain rights in this invention. Field of the Invention
[0005] The present invention relates to a safe and energy-efficient direct regeneration process for lithium-ion battery cathodes.
[0006] background
[0007] Lithium-ion batteries (LIBs) are widely used power sources for portable electronic devices, recreational equipment, and electric vehicles (EVs) due to their high energy density and long cycle life. Due to an average lifespan of 5-10 years, a large number of LIBs will be retired in the next few years. It is estimated that by 2025, about 1 million EV batteries will reach their end of life (EOL), which may cause major problems if they are not properly handled. The release of flammable and hazardous wastes (such as electrolytes and transition metals) caused by improper disposal of waste LIBs can contaminate soil, water, and air. Therefore, it has become an urgent need to develop effective and environmentally friendly LIB recycling strategies, not only to reduce the environmental impact of LIB waste, but also to recover valuable resources, such as lithium (Li), and cobalt (Co) and nickel (Ni).
[0008] Recently, due to the high value of Co, Ni and Li, the recycling of LIB cathodes has received great attention. Existing methods use three main recycling methods: pyrometallurgical recycling, hydrometallurgical recycling and direct recycling. The pyrometallurgical process is based on a high-temperature smelting process, which usually involves burning mixed LIB materials, followed by chemical separation. The process is characterized by low operational complexity and easy expansion and development, but has a relatively low recovery efficiency. Aqueous chemistry is usually used in the hydrometallurgical process, which involves leaching in acid, followed by precipitation, chemical separation and purification. Although pyrometallurgical and hydrometallurgical processes represent the most advanced technologies in the recycling industry, the involvement of high-temperature smelting and the extensive use of acid chemicals and alkali chemicals have respectively caused concerns about large-scale energy consumption (and high operating costs) and secondary pollution. The combination of pyrometallurgical recycling methods and hydrometallurgical recycling methods provides some benefits in reducing energy and reagent costs while improving recovery efficiency. The latest advance in pyrometallurgy is a closed-loop "hydro-to-cathode" method that eliminates the complex chemical separation of Ni, Co and Mn, providing battery recycling efficiency and lower operating costs. However, these methods require the complete decomposition of cathode particles (e.g., NCM) into their elemental products (e.g., CoSO4, NiSO4, Li2CO3), which wastes a large amount of embedded energy in the cathode particle structure. In contrast, direct recycling methods involve a physical separation process to harvest cathode and anode materials, in which mild post-treatment is used to repair the compositional and structural defects of the electrode particles while retaining their original compound structure and embedded energy. In this regard, direct recycling appears to offer the greatest potential for maximizing the value recovered from LIBs.
[0009] In recent years, many researchers in this field have reported direct LIB cathode regeneration based on hydrothermal relithiation followed by a rapid post-annealing step, demonstrating the regeneration of spent LiCoO2 (LCO), LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2The morphology, composition and crystal structure of O2 (NCM622) and LiFePO4 (LFP) cathodes were effectively reconstructed, resulting in the same level of electrochemical performance as their original materials. See, for example, E. Gratz et al., “A closed loop process for recycling spent lithium ion batteries”, Journal of Power Sources 262 (2014) 255-262; Y. Shi et al., “Ambient-Pressure Relithiation of Degraded Li x Ni 0.5 Co 0.2 Mn 0.3"O2(0 < x < 1) via Eutectic Solutions for Direct Regeneration of Lithium-Ion Battery Cathodes", Adv. Energy Mater. 9 (2019) 1900454; S. Sloop et al., "A direct recycling case study from a lithium-ion battery recall", Sustainable Materials and Technologies 25 (2020) e00152; L. Brückner et al., "Industrial Recycling of Lithium-Ion Batteries—A Critical Review of Metallurgical Process Routes", Metals 10 (2020) 1107; Y. Shi et al., "Effective regeneration of LiCoO2 from spent lithium-ion batteries: A direct approach towards high-performance active particles", Green Chem. 20 (2018) 851–862; and P. Xu et al., "Efficient Direct Recycling of Lithium-Ion Battery Cathodes by Targeted Healing", Joule 4 (2020) 2609–2626. The described methods are characterized by simple operation and low energy consumption, which utilize a hydrothermal relithiation process to recycle the cathode composition without involving variations in Li loss in different feedstocks of degraded LIBs. These processes also utilize a rapid sintering process to restore the cathode microstructure with a desirable stoichiometry and crystallinity. However, a hydrothermal relithiation temperature greater than 200 °C (e.g., 220 °C) is typically required to fully restore Li defects to achieve good electrochemical properties. Due to the high vapor pressure inside the relithiation reactor (e.g., 25 bar at 220 °C), such a wet relithiation process poses potential safety issues for large-scale operation. Therefore, there is still a need for a safe and energy-efficient hydrothermal relithiation process for effective direct recycling of LIBs.
[0010] Overview
[0011] The method of the present invention provides a process for waste LiNi x Co y Mnz A safe and energy-efficient direct regeneration process for O2 (0 < x, y, z < 1, x + y + z = 1, or NCM) cathode materials based on low-temperature hydrothermal relithiation (LTHR) at ambient pressure. A low-concentration, low-cost redox mediator is used to improve the relithiation kinetics of waste NCM materials, which enables the complete relithiation temperature to be reduced from 220 °C to 100 °C or lower. The pressure generated during the relithiation process can be reduced from ~25 bar to 1 bar, significantly improving operational safety.
[0012] The effectiveness of the improved method has been demonstrated on different NCM materials, including chemically delithiated NCM111, cycled (degraded) NCM111, and cycled NCM622, which have been successfully regenerated and fully restored their composition, crystal structure, and electrochemical properties, achieving the same effectiveness as that achieved in high-temperature processes.
[0013] The method of the present invention provides a general low-temperature hydrothermal relithiation (LTHR) process to efficiently and safely recover the Li composition of degraded NCM cathode materials at ambient pressure. An important aspect of the process of the present invention is the use of a class of reducing agents as green additives (GAs) in a low-concentration (1% - 3% v / v) aqueous relithiation solution (LiOH solution). These additives allow the hydrothermal relithiation temperature to be reduced while correspondingly reducing the processing pressure. The LTHR process of the present invention exhibits the same effectiveness in relithiation as that achievable with high-temperature processes, resulting in the complete regeneration of chemically delithiated NCM111, cycled NCM111, and cycled NCM622. This LTHR process can pave the way for more sustainable LIB recycling with high economic returns, high operational safety, and lower costs.
[0014] In one aspect of the present invention, a method for regenerating a spent lithium-ion battery cathode material, where the cathode material is in powder form, includes the steps of processing the cathode material in an aqueous lithium (Li) solution and a reducing agent at a temperature in the range of 80 °C to 100 °C for a processing time period; washing and drying the processed cathode material; annealing the dried processed cathode material in oxygen at an annealing temperature for an annealing time period to produce a regenerated cathode material. In some embodiments, the lithium solution is LiOH, and the solution can be 0.1 M to 4 M LiOH with 1% (v / v) - 3% (v / v) of a reducing agent. Preferably, the reducing agent is a green reducing additive, which can be one or a combination of ethanol (ET), ethylene glycol (EG), and hydrogen peroxide (HP). The processing time period can be from 2 hours to 20 hours, more preferably 6 hours to 12 hours, and most preferably 8 hours. The annealing temperature can be in the range of 600 °C to 1000 °C and the annealing time period is from 1 hour to 10 hours, and more preferably can be 850 °C, where the annealing time period is 4 hours. The cathode material can be LiNi x Co y Mn z O2, where 0 < x, y, z < 1, x + y + z = 1 (“NCM”), which can be LiNi 0.33 Co 0.33 Mn 0.33 O2 (NCM111) or LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622). In some embodiments, 5 mol% of an excess of Li2CO3 can be mixed with the processed cathode material before annealing.
[0015] In another aspect of the present invention, a method for treating a lithium-ion battery cathode material from spent battery cells includes: separating a cathode strip from the battery cells; treating the cathode strip in one or more solvent solutions to remove NCM, binder, and carbon black from the cathode strip matrix and extract NCM powder; processing the NCM powder in an aqueous lithium (Li) solution and a reducing agent at a temperature in the range of 80 °C to 100 °C for a processing period to relithiate the NCM powder; washing and drying the relithiated powder; and annealing the dried powder in oxygen at an annealing temperature for an annealing period to produce a cathode powder having a restored composition, crystal structure, and electrochemical performance. The method may further include mixing 5 mol% excess Li2CO3 with the relithiated powder prior to annealing. In some embodiments, the lithium solution is LiOH, and the solution may be 0.1 M to 4 M LiOH with 1% (v / v) - 3% (v / v) of the reducing agent. Preferably, the reducing agent is a green reducing additive, which may be one or a combination of ethanol (ET), ethylene glycol (EG), and hydrogen peroxide (HP). The processing period may be from 2 hours to 20 hours, and more preferably 6 hours to 12 hours. The annealing temperature may be in the range of 600 °C to 1000 °C and the annealing period is from 1 hour to 10 hours, and more particularly may be 850 °C, where the annealing period is 4 hours. The cathode material may be LiNi x Co y Mn z O2, where 0 < x, y, z < 1, x + y + z = 1 (“NCM”), which may be LiNi 0.33 Co 0.33 Mn 0.33 O2 (NCM111) or LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622). BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1A-Figure 1C A profile of the relithiation process of degraded NCM111 according to an embodiment of the method of the present invention is provided, where Figure 1A is a schematic diagram of a direct regeneration process of a degraded NCM material based on hydrothermal relithiation; Figure 1B illustrates the role of GA in the LTHR process of the present invention; and Figure 1C compares the saturated vapor pressure of water at temperatures associated with different reactor processing conditions.
[0018] Figure 2 is a flowchart of a process showing an exemplary material harvesting process for recycling spent LIBs.
[0019] Figure 3 is a flow chart illustrating a process for direct recycling of LIBs according to an embodiment of the present invention.
[0020] Figure 4A-4F The relithiation kinetics are shown in Figure 2. Figure 4A The Li contents in different NCM111 particles with and without relithiation obtained by ICP results were compared; Figure 4B The composition evolution of cycled NCM111 during relithiation via the LTHR process was plotted; Figure 4C The XRD patterns of cathode samples relithiated with three different GAs (ET, EG, and HP) at 100 °C and the control sample (T-NCM111) were plotted; Figure 4D The unit cell parameters a and c of different NCM111 samples are plotted; Figure 4E and Figure 4F XRD patterns of the samples relithiated at 100 °C and the control samples (T-NCM111 and D-NCM111), respectively.
[0021] Figure 5A and Figure 5B Here are the SEM images of different samples: Figure 5A (Panel a) Cycled NCM111, (Panel b) T-NCM111, (Panel c) relithiated without green additive, (Panel d) relithiated in the presence of hydrogen peroxide, (Panel e) relithiated in the presence of ethanol, and (Panel f) relithiated in the presence of ethylene glycol at 100 °C. Scale bar in each panel is 10 μm; Figure 5B (Panel a) Cycled NCM111, (Panel b) T-NCM111, (Panel c) relithiated without green additive, (Panel d) relithiated with hydrogen peroxide, (Panel e) relithiated with ethanol, and (Panel f) relithiated with ethylene glycol at 100°C. Scale bar in each panel is 4 μm.
[0022] Figure 6A-6D The XPS spectra of different NCM111 samples in the Ni 2p region at 100 °C, without GA and with GA, respectively. Fig. 6A C-NCM111 is shown. Figure 6B T-NCM111 is shown, and Figure 6C and Fig.6D Relithiated C-NCM111 is shown.
[0023] Figure 7A-7HThe electrochemical performance of HS-C-NCM111 and HS-C-NCM622 is shown in Figure 2. Fig. 7A and Figure 7B The voltage profile and cycling stability of NCM111 samples regenerated with different GAs at 100 °C and their comparison with pristine C-NCM111 and untreated C-NCM111 are shown respectively; Figure 7C and Figure 7G The cycling stability of pristine NCM111 and regenerated NCM111 are plotted; Fig.7D and Fig. 7E The voltage profiles and cycling stability of the regenerated NCM622 sample, the untreated NCM622 sample, and the original NCM622 sample, respectively; Figure 7F and Figure 7H The cycling stabilities of the pristine NCM622 sample and the regenerated NCM622 are plotted.
[0024] Fig. 8A and Figure 8B The voltage profiles and cycling stability performance of NCM111 regenerated at 90 °C and 100 °C as well as control samples (T-NCM111 and D-NCM111) are plotted, respectively.
[0025] Figure 9A-9B The full-cell cycling stabilities of HS-C-NCM111 and HS-C-NCM622 regenerated using EG as a reductant are shown, respectively.
[0026] Figure 10A-10B XRD patterns of cycled samples T-NCM111, HS-EG and HS-No GA (HS-No GA) in the scanning ranges of 10°-80° and 18°-19° are shown, respectively.
[0027] Figure 11A-11B The energy consumption and GHG emissions of direct recycling methods based on different processing temperatures are compared.
[0028] Fig.12 The energy consumption, GHG emissions, costs and benefits of the pyrometallurgical ("Pyro"), hydrometallurgical ("Hydro") and LTHR-based direct ("Direct") recycling processes of NCM111 are compared.
[0029] Detailed description of implementation plan
[0030] Figure 1A-Figure 1C An overview of the LTHR relithiation process according to the scheme of the present invention is provided. A simple flow chart of the process is shown in Figure 3. According to the redox-mediated LTHR process for direct recycling of the present invention, the degraded NCM111 particles 200 are treated by relithiation in a LiOH solution with the addition of different reducing agents (step 202). In order to meet the important objectives of the process of the present invention, especially the important objective of reducing / eliminating the need for environmentally unfriendly materials, the reducing agent used is a green additive or "GA". In the process of the present invention, the key to effectively regenerating the degraded NCM111 at low temperature is to convert the Ni in the degraded NCM111 into a re-lithiation catalyst. 3+ Ion reduction to Ni 2+ ions and compensate for the Li deficiency in the structure for charge balance. The method of the present invention uses a reducing environment to help lower the activation barrier, which can promote Ni 3+ The restoration of Figure 1A The solution treatment method uses a reducing agent to promote an oxidation-reduction reaction in which Ni in the crystal is reduced by the donation of electrons from the reducing agent. 3+ ions can be reduced more easily. Therefore, Ni 3+ The mild reduction of Li + inserted into the cathode material, which is consistent with the electrochemical Li + Insertion has the same essence ( Figure 1B ). Three different GAs (ethanol, hydrogen peroxide, and ethylene glycol) are believed to demonstrate this mechanism, however, as will be appreciated by those skilled in the art, additional GAs are known and can be used to provide the desired redox properties, including but not limited to glycerol, citric acid, L-ascorbic acid, and other known green reductants. In addition, combinations of GAs may also be used. Of the three GAs discussed herein, the standard reduction potentials are -0.77 V (ethanol, relative to standard hydrogen electrode or SHE), 0.15 V (hydrogen peroxide), and -0.72 V (ethylene glycol), respectively, all lower than Ni 3+ / Ni 2+ Redox potential (~0.7 V). Gibbs free energy of reaction between NMC material and GA, ΔG = -nFE = -nF (0.7 -E GA ), is negative, which indicates that the relithiation of the degraded NCM material with GA is thermodynamically favorable. In order to detect the oxidation products of the three reducing agents in the LiOH solution after the hydrothermal process, the NMR spectrum was measured, and the NMR spectrum showed that the oxidation products of ethanol, hydrogen peroxide and ethylene glycol in the LiOH solution were lithium acetate, oxygen and lithium oxalate, respectively, wherein the following reactions occurred:
[0031]
[0032]
[0033] Therefore, due to improved redox kinetics, reducing additives allow relithiation to be performed at relatively low temperatures and pressures, which reduces energy costs and improves operational safety ( Figure 1C ). Although all three GAs can help regenerate NMC, ethylene glycol (EG) is considered the most suitable for practical application due to its relatively low cost and safety considerations (high flash point and boiling point). Although further evaluation included all three GA candidates, EG was mainly used as a reducing agent to study the mechanism of the LTHR process.
[0034] To further evaluate the effectiveness of the LTHR method of the present invention, two types of degraded NCM111 particles were initially used to study the redox-mediated effects. One is D-NCM111 with 10% lithium loss, which is a model material from the ReCell project; and the other is C-NCM111 from Honda Clarity EV. D-NCM11 was used for preliminary screening of GAs, and then a system dynamics study was performed on C-NCM111. Specifically, with the assistance of three different GAs including ethanol (ET), ethylene glycol (EG) and hydrogen peroxide (HP), C-NCM111 was subjected to relithiation at 100°C in a 4M LiOH solution for 8 hours, followed by rapid annealing at 850°C. As a further verification of the key role of the reducing agent, C-NCM111 was treated with a LiOH solution without a reducing agent under the same conditions.
[0035] Chemically delithiated NCM111 with ~10% Li loss, denoted as "D-NCM111", was made by the Materials Engineering Research Facility (MERF) at Argonne National Laboratory. Briefly, the original NCM111 (provided by Toda America Inc.) was reacted with an aqueous solution of potassium persulfate to leach Li. The leached material was then washed with water, then with acetonitrile, and finally dried under vacuum at ambient conditions. This delithiated NCM111 was used as our starting material for additive screening and was manufactured in batch sizes of 1 kg each.
[0036] Reference Figure 2 , showing a process flow for obtaining materials for evaluating degradation of the process of the present invention. Starting from step 100, Commercial NCM111 batteries (20Ah) were disassembled in the Clarity Hybrid EV and separated into three main components: housing and electrolyte (step 102), cathode strips (step 104) and anode strips and separators (step 106). In order to harvest the NCM111 material (denoted as "C-NCM111") of the electrochemical cycle, the cathode strips from step 104 were rinsed with dimethyl carbonate (DMC) to eliminate the remaining electrolyte. After drying, the cathode strips were soaked in N-methyl-2-pyrrolidone (NMP) (step 108), and then ultrasonic treatment was continued for 20 minutes to remove NCM powder, binder and carbon black (CB) from the aluminum matrix. The obtained solution was centrifuged at 3,500rpm for 5 minutes to extract C-NCM111 powder. The precipitate was rinsed with NMP several times, then collected and dried for regeneration experiments. CB has a significantly lower density than NCM111 and can be separated by gravity during the precipitation process. A similar approach was used to isolate electrochemically cycled NCM622 (C-NCM622), also from Argonne National Laboratory, with significant capacity fade.
[0037] Mentioned again Figure 3 , the degraded cathode powder 200 (chemically delithiated NCM111 and electrochemically degraded NCM111 and NCM622) is stirred in an aqueous LiOH solution to which 1% (v / v)-3% (v / v) of a reducing agent, in particular a green additive (GA) is added (step 202), and the degraded cathode powder 200 is treated at 80°C-100°C (step 204) for 2 hours to 20 hours ("processing period") for relithiation. The LiOH solution can have a concentration in the range of 0.1M-4M. In most tests, a LiOH concentration of 4M, a temperature of 100°C and a processing period of 8 hours were used. This step is followed by washing with deionized water to remove Li salt residues. After drying, the relithiated powder is mixed with 5 mol% excess Li2CO3 (to compensate for Li loss during the post-annealing process) and undergoes "rapid annealing". (As is known in the art, a "rapid anneal" is distinguishable from a "full anneal" in terms of conditions and resulting material changes.) The annealing parameters used during most evaluations were 850°C in oxygen for 4 hours with a ramp rate of 5°C min -1(Step 206) to produce a regenerated cathode material (step 208). In summary, the "rapid annealing" conditions used in the process of the present invention can vary from a temperature of about 600°C to 1,000°C, within a range of 1 hour and 10 hours. It is worth noting that transition metal leaching may occur during long cycles, especially under harsh conditions used for spent cathodes. The extent of leaching is affected by the cycle conditions (temperature, upper cutoff voltage, etc.), the microstructure of the cathode, the type of cathode material (especially the Mn-rich type), etc. However, in the current case with NCM, transition metal leaching is not considered to be a significant problem. Based on the ICP results, no obvious changes in transition metal composition and dissolution of transition metal ions were found in the spent NCM compared to comparable original materials. The amount of transition metal leaching is extremely small.
[0038] The chemical composition of various cathode powders was evaluated by inductively coupled plasma mass spectrometry (ICP-MS, Thermo Scientific, iCAP RQ model). The surface composition of the samples was analyzed by X-ray photoelectron spectroscopy (XPS). XPS data were collected using a PHI 5000VersaProbe II system (Physical Electronics) with Al Kα radiation (1486.6 eV). X-ray powder diffraction (XRD) with a Bruker D2 phase analyzer was used to determine the crystal structure. The XRD results were subjected to Rietveld refinement using the General Structure Analysis System (GSAS) software with the EXPGUI interface. Scanning electron microscopy (SEM, FEI XL30) was used to examine the surface structure and morphology of various cathode particles.
[0039] By having ∼10 mg cm -2The electrochemical performance of all samples was evaluated by using a coin cell (half cell) with a cathode mass load of 10000. In order to prepare the slurry of the electrode, the original NCM cathode material, the degraded NCM cathode material or the regenerated NCM cathode material were mixed with a conductive agent (Super P65) and a polyvinylidene fluoride (PVDF) adhesive in a mass ratio of 8:1:1 in N-methyl-2-pyrrolidone (NMP) solvent. Then, the slurry was distributed (cast) on an aluminum foil with a scraper, and then, dried in a vacuum oven at 120°C for 12 hours. The dried laminate was cut into a disc shape and calendered. Coin cells were fabricated in a glove box with a lithium metal disk (thickness 1.1 mm) as the counter electrode, LP40 (1 M LiPF6 in ethylene carbonate / diethyl carbonate = 50:50 (v / v)) or Gen2 (1.2 M LIPF6 in EC / EMC = 3:7) as the electrolyte, and a three-layer membrane (Celgard 2320) as the separator. Constant current charge and discharge were tested in the potential range of 3.0 V-4.3 V using a Neware battery cycler, with 4 activation cycles at a rate of C / 10, followed by 50 cycles at a constant rate of C / 3.
[0040] Figure 4A-4F The relithiation kinetics according to the method of the present invention are shown in FIG. Figure 4A As shown in the ICP-MS results, C-NCM111(x Li =0.62) of Li content (x Li ) was successfully recovered after the regeneration process with GA at 100 °C (x Li =1.06), which maintains the same stoichiometry as T-NCM111 (x Li =1.06). Each of the three GAs (ET, HP, and EG) showed almost the same effect on composition recovery. In contrast, without GA, the Li content could only reach 0.98 under the same conditions. This effect was also observed in the case of D-NCM111, where the Li content was restored from 0.9 to 1.06 with GA (see Table 1 below). In addition, we evaluated the relithiation kinetics of composition recovery for the LTHR process ( Figure 4B ). With the assistance of GA, the 8h-LTHR process at 100°C can achieve the same 100% composition recovery as the conventional 220°C process (see, e.g., Figure 1C ).
[0041] The morphology of the regenerated samples and the control samples were further compared. The LTHR process did not show any effect on the particle morphology ( Figure 5A-Figure 5B), which may be attributed to the mild regeneration conditions. XRD results also confirmed the effectiveness of the LTHR process in restoring the crystal structure of C-NCM111 and D-NCM111 samples ( Figure 4C-4F ). In conclusion, the diffraction peaks of all samples are similar to those with The space group matches well with the typical α-NaFeO2 structure, indicating that the bulk structure of NCM111 is not affected by electrochemical cycling (C-NCM111), chemical delithiation (D-NCM111), and our regeneration strategy, which once again demonstrates the feasibility of the direct regeneration process based on LTHR.
[0042] During the entire regeneration process, the evolution of the microstructure is clearly observed. C-NCM111 shows a shift to a lower (003) peak ( Figure 4D ), which can be achieved by + The increase in the spacing between the peaks in the (108) / (110) doublet indicates a decrease in the a lattice parameter, which is due to the increase in the electrostatic repulsion between the oxygen layers along the c direction when N is deficient. 2+ Compared with Ni 3+ The smaller effective ionic radius of NCM111 leads to a decrease in the average metal-metal distance. A similar peak shift can also be observed in D-NCM111 ( Figure 4E-4F ). The lattice parameters of a and c unit cells were determined by Rietveld refinement and are listed in Table 1.
[0043]
[0044]
[0045] Table 1
[0046] a lattice parameter from (T-NCM111) are reduced to (C-NCM111) and (D-NCM111). c Lattice parameters from (T-NCM111) respectively increased to (C-NCM111) and (D-NCM111), which is consistent with the peak shift from the XRD results. After the LTHR process, the (003) peak, (108) peak, and (110) peak obviously shifted back to the original positions in the original T-NCM111, indicating the restoration of the original microstructure ( Figure 4D and Figure 4F ). The lattice parameters of the regenerated samples a and c are close to that of T-NCM111, indicating that despite the low relithiation temperature, Li +ions reached their equilibrium state in the lattice structure. In addition, the Li / Ni mixing ratio of C-NCM111 decreased from 5.47 to 2.40 (ET), 2.43 (HP), and 2.41 (EG), respectively ( Figure 4E ), reaching a mixing ratio that is almost the same as that of pristine T-NCM111 (2.39). In contrast, the Li / Ni mixing ratio did not fully recover to its original state without GA, which again demonstrated that GA is beneficial for regenerating NCM111 in the LTHR process.
[0047] To further understand the role of GA in the LTHR process, XPS measurements were performed to determine the valence states of Ni in different NCM111 before annealing ( Figure 6A-6D ). 3+ / Ni 2+ The lower redox voltage of C-NCM111 is expected to cause only a change in Ni valence state, since the maximum Li deficiency is only 0.4 in this case. 40.78% of Ni is observed to be Ni in C-NCM111. 3+ in the form of Fig. 6A After relithiation in a solution containing only LiOH ( Figure 6C ), ~21.07% Ni in Ni 3+ This is consistent with the fact that in the presence of GA, i.e., LiOH+GA, nearly 100% Ni 3+ Reduced to Ni 2+ In this case, H2O is used as a weak reducing agent to convert Ni 3+ Reduction to Ni 2+ In contrast, in the presence of GA, all Ni 3+ Reduced to Ni by LTHR process 2+ , indicating significantly improved relithiation kinetics. Similar results were observed for D-NCM111, where relithiation in GA-containing LiOH solutions was more efficient than that in LiOH without GA. Specifically, 24.68% Ni 2+ Converted to Ni due to chemical delithiation 3+ After LTHR treatment without GA, 22.79% Ni was still present in the form of Ni 3+ This means that only 1.89% Ni 3+ is spontaneously reduced to Ni 2+ These results confirm that GA plays an important role in promoting Ni 3+ Reduction to Ni 2+ This further promoted the importance of Li + The Li-deficient sites in the NCM cathode are intercalated from the solution to compensate the charge.
[0048] The electrochemical performance of C-NCM111 regenerated by LTHR process followed by rapid annealing at 850° C. (denoted as “HS-C-NCM111”) was evaluated by half-cell tests. Figure 7A-7B The voltage profiles and cycling stability of various materials and processing conditions are plotted. C-NCM111 exhibits 51 mAh g -1 The initial capacity of Ni 3+ The effective ionic radius is smaller than that of Ni 2+ , when Li is in a deficient state, Ni 3+ It is easier to occupy the Li site, and the cation mixing ratio increases accordingly. High cation mixing will prevent Li + transport, which reduces Li + Storage capacity and rate performance. After regeneration, the regenerated and pristine samples exhibited ~155 mAh g in Gen2 electrolyte at C / 10. -1 The C-NCM111 treated without GA showed only 92% capacity retention after 60 cycles at C / 3. In contrast, the regenerated NCM111 from the LTHR process with different GAs all maintained a similar capacity retention of ~96% after 60 cycles at C / 3, showing the same cycling stability as the original T-NCM111. A similar trend was also observed in the D-NCM111 sample with LP40 in the half-cell.
[0049] D-NCM111 exhibits 134.0 mAh g at C / 10 -1 After LTHR and subsequent rapid annealing, the initial capacity of HS-D-NCM111 reaches 154 mAh g at C / 10. -1 , and after 50 cycles at C / 3, the capacity retention rate increased to 91%, which is comparable to that of the original T-NCM111. 2 Half-cell tests were evaluated at high loads of 3 mg / cm. Under this condition, the cycling performance is limited by the poor stability of the lithium metal anode. 2 The rate capability and half-cell performance (200 cycles at 1C) of HS-C-NCM111-GA (with EG) were evaluated at the cathode loading ( Figure 7C , Figure 7G ). After 200 cycles, HS-C-NCM111-GA provided 141 mAh g at 1C. -1The capacity of HS-C-NCM111-GA was 157 mAh g at 0.1C, 0.3C, 1C, 3C, and 5C. -1 , 151mAh g -1 , 140mAh g -1 、130mAhg -1 , 113mAh g -1 The capacity of the original T-NCM111 reached 156mAh g at 0.1C, 0.3C, 1C, 3C, and 5C. -1 , 151mAh g -1 , 140mAh g -1 , 129mAh g -1 , 113mAh g -1 These results indicate that the rate capacity of the regenerated NCM111 has been restored. Full cell tests of HS-C-NCM111-GA paired with a graphite anode were also performed (cathode loading: 10 mg / cm 2 ).like Fig.9A As shown in the full battery test, HS-C-NCM111-GA exhibited 138 mAh g at 1C. -1 The initial capacity is 120 mAh g after 100 cycles. -1 The capacity of HS-C-NCM111-GA is comparable to that of the original T-NCM111 under the same conditions. In rate, half-cell and full-cell tests, HS-C-NCM111-GA can achieve the same electrochemical performance as that of T-NCM111, which confirms the success of the regeneration method of the present invention.
[0050] In addition, Fig. 8A and Figure 8B In Figure 2, the delithiated NCM111 regenerated by LTHR process at 90 °C and 100 °C followed by rapid annealing are denoted as “HS-D-NCM111-GA-90 °C” and “HS-D-NCM111-GA-100 °C”. The initial capacity of HS-D-NCM111-GA-90 °C reaches 154.0 mAh g at C / 10. -1 , reaching the same level of capacity as the original NCM111. In addition, HS-D-NCM111-GA-90℃ provided 149.8mAh g -1 The initial capacity of , and after 50 cycles, the capacity retention can reach 91%, which is comparable to the original level (T-NCM111). This result shows that the sample is effectively recovered after hydrothermal treatment at 100 ° C or even lower temperatures followed by annealing.
[0051] In view of the growing interest in high-Ni NCM cathodes, the tests were extended to NCM622 (C-NCM622) by comparing the electrochemical properties between cycled samples (C-NCM622), LTHR-regenerated samples (denoted as HS-C-NCM622), and pristine samples using Gen2 electrolyte. Figure 7D-7F , Figure 7H As mentioned previously, while all three GAs regenerate NMC111 well, EG is considered the most suitable for practical applications due to its low cost and safety benefits. Therefore, for the extended testing of NCM622, EG was used as the reducing agent for the LTHR process.
[0052] C-NCM622 exhibits 121 mAh g at C / 10 -1 The initial capacity of HS-C-NCM622 reaches 175 mAh g at C / 10 through LTHR process and rapid annealing. -1 , and after 60 cycles at C / 3, the capacity retention is improved to 92%, which is equal to that of the original T-NCM622. To demonstrate the electrochemical performance of the regenerated NCM622, we evaluated the 2 Rate performance and cycling stability of a half-cell (200 cycles at 1C) of a cathode-loaded HS-C-NCM622-GA (regenerated with EG as GA) ( Figure 7F , Figure 7H HS-C-NCM622-GA provides similar rate capacity and long cycle stability to those of T-NCM622. In the case of HS-C-NCM622-GA paired with a graphite anode (cathode loading: 10 mg / cm 2 ) in full battery test ( Fig. 9B ). In the full cell test, HS-C-NCM622-GA showed 154 mAhg in the first cycle at 1C. -1 The capacity of the battery was 130 mAh g after 100 cycles at 1C. -1 , which is close to the capacity of the original T-NCM111 under the same conditions. In summary, HS-C-NCM622-GA can achieve the same electrochemical performance as T-NCM622 in rate tests, half-cell tests, and full-cell tests, thus confirming the success of NCM622 regeneration. The successful regeneration of both NCM111 and NCM622 using different GAs demonstrates the high efficiency and versatility of the LTHR-based direct recycling method of the present invention. Overall, these results support the use of a reducing environment to reduce Ni 3+Activation barriers for reduction and relithiation.
[0053] To examine the differences in structural stability between the recycled and pristine materials, the HS-EG electrode, HS-without GA electrode, and T-NCM111 electrode after cycling (denoted as “cycled HS-EG,” “cycled HS-without GA,” and “cycled T-NCM111,” respectively) were characterized by XRD ( Figure 10A-10B ). The XRD diffraction peaks of these samples still match well with the typical layered structure without major impurity phases, indicating that the bulk structure of the original NCM111 and the regenerated NCM111 is not affected by electrochemical cycling. No obvious structural differences were observed between the cycled HS-EG and the cycled T-NCM111, which also proves the feasibility of the direct regeneration process based on LTHR. However, as previously discussed, in the absence of GA addition, the Li content, Li / Ni mixing ratio, transition metal valence, electrochemical stability, etc. of the regenerated material cannot be fully restored to the original state. After cycling, the (003) peak of the cycled HS-without GA shifts to a lower degree compared to the cycled HS-EG and the cycled T-NCM111, which is due to more severe Li deficiency and more significant lattice expansion along the c-axis. In summary, this once again proves that GA is beneficial to regenerate NCM111 in the LTHR process to maintain structural stability, and proves the recovery effect to a certain extent.
[0054] In conventional hydrothermal relithiation processes, NCM materials require a high pressure reactor (usually an autoclave) to maintain a pressure greater than 25 bar (the saturation pressure of water) at 220 °C (see Figure 1C ). Using the method of the present invention, the kinetics of relithiation can be promoted by GA, and LTHR can be carried out at a temperature equal to or below the boiling point of water, allowing the relithiation process to be carried out at ambient pressure, thereby eliminating the need for a high-pressure reactor. Specifically, when the relithiation temperature is reduced to 100°C, the pressure required for the LTHR process of the present invention can be reduced to about 1 bar. By replacing traditional high-pressure reactors with low-cost vessels, large-scale direct regeneration becomes more feasible for industrial applications without the need for additional safety precautions required by previous processes.
[0055] The environmental and economic impacts of direct regeneration based on LTHR were evaluated using the EverBatt model developed by Argonne National Laboratory using a volume of 10,000 tons of spent LIBs per year. Fig.11A ), greenhouse gas (GHG) emissions ( Fig. 11BA life-cycle analysis (LCA) of the entire direct recycling process of LTHR and conventional high-pressure reaction was conducted in terms of energy consumption, operating costs and total benefits. By assuming the same pre-treatment and post-separation, the modeling results show that the total energy consumption is increased from 5.28 MJ kg of spent batteries for conventional high-pressure regeneration reaction to 5.28 MJ kg of spent batteries for conventional high-pressure regeneration reaction. -1 Reduced to only 4.22MJ kg of waste batteries for LTHR -1 ( FIG. 5 , panel a) Consistently, the direct regeneration process using LTHR can also reduce GHG emissions by about 0.03 kg per kg of battery compared to the conventional high-pressure regeneration reaction at 220° C.
[0056] Due to the reduced temperature of the relithiation process, low-quality industrial waste heat can potentially be used to provide heat to the LTHR process. The total process cost of direct recycling of NCM batteries is estimated to be $2.07 and $2.25 for spent battery cells processed at 100°C and 220°C, respectively. Therefore, regenerated cathode production using LTHR is expected to provide an additional benefit of $0.18 per kg of spent battery. In addition, significant cost savings can be achieved due to reduced safety requirements.
[0057] The LTHR-based direct recycling method for NCM recycling of the present invention was also compared with conventional pyrometallurgical recycling and hydrometallurgical recycling processes using LCA. Fig.12 The results of this comparison are provided. The energy consumption of the pyrometallurgical recycling process and the hydrometallurgical recycling process of spent NCM batteries are 18.497 MJ kg -1 and 30.710MJkg -1 , which is significantly higher than only 4.166 MJ kg -1 LTHR-based direct recycling process (Panel a). As shown in Panel b, for 1 kg of spent NCM batteries, pyrometallurgy (2.457 kg) and hydrometallurgy (2.258 kg) released significantly higher GHGs than the direct recycling method (0.577 kg). These can be explained by the high temperature smelting in the pyrometallurgical process and the generation of a large amount of chemicals used in the hydrometallurgical recycling process. In addition, the costs and benefits associated with the three recycling processes were modeled and analyzed, such as Fig.12As shown in panels c and d in the figure. The total costs of pyrometallurgical recycling, hydrometallurgical recycling and LTHR-based direct recycling of 1 kg of spent NCM batteries are $3.10, $2.54 and $2.04, respectively. This is due to the expensive equipment, large-scale use of chemicals and high energy consumption of the pyrometallurgical recycling and hydrometallurgical recycling processes. Since Ni and Co are very valuable, 1 kg of spent NCM batteries can still earn $2.16 and $3.07 respectively through pyrometallurgical recycling and hydrometallurgical recycling. Due to the significant reduction in total energy use, GHG emissions and processing costs, the LTHR-based direct regeneration method of the present invention is a preferred option for closed-loop and safe LIB recycling. In general, the LTHR-based direct recycling method meets each element of the "4H" method for battery recycling: high efficiency, high economic return, high environmental benefits and high safety, which represents a new trend in sustainable LIB recycling.
Claims
1. A method for regenerating spent lithium-ion battery cathode material, wherein the cathode material is in powder form, the method comprising: processing the cathode material in an aqueous lithium (Li) solution and a reducing agent at a temperature in a range of 80° C. to 100° C. for a processing period sufficient to relithiate the cathode material; washing and drying the processed cathode material; and The dried processed cathode material is annealed in oxygen at an annealing temperature for an annealing period to produce a regenerated cathode material.
2. The method of claim 1, wherein the lithium solution is LiOH. The method according to claim 1 , wherein the reducing agent is a green reducing additive. 4 . The method according to claim 3 , wherein the green reducing additive is one of ethanol (ET), ethylene glycol (EG) and hydrogen peroxide (HP) or a combination thereof.
5. The method of claim 1, wherein the processing time period is from 2 hours to 20 hours. 6 . The method of claim 1 , wherein the annealing temperature is in the range of 600° C. to 1000° C., and the annealing time period is from 1 hour to 10 hours.
7. The method of claim 6, wherein the annealing temperature is 850°C and the annealing time period is four hours.
8. The method according to claim 1, wherein the cathode material is LiNi x Co y Mn z O2, where 0 <x、y、z<1,x+y+z=1(“NCM”)。 9. The method of claim 8, wherein the NCM is LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111).
10. The method of claim 8, wherein the NCM is LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622).
11. The method of claim 1, wherein the aqueous lithium solution is 0.1 M to 4 M LiOH with 1% (v / v) - 3% (v / v) of the reducing agent.
12. The method of claim 1, further comprising mixing 5 mol% excess Li2CO3 with the processed cathode material prior to annealing.
13. A method for processing lithium ion battery cathode material from spent battery cells, comprising: separating cathode strips from said battery cells; treating the cathode strip in one or more solvent solutions to remove NCM, binder and carbon black from the cathode strip substrate and extract NCM powder; processing the NCM powder in an aqueous lithium (Li) solution and a reducing agent at a temperature in a range of 80° C. to 100° C. for a processing period sufficient to relithiate the NCM powder; washing and drying the relithiated powder; and The dried powder is annealed in oxygen at an annealing temperature for an annealing period to produce a cathode powder having restored composition, crystal structure, and electrochemical properties.
14. The method of claim 13, further comprising mixing 5 mol% excess Li2CO3 with the relithiated powder prior to annealing.
15. The method of claim 13, wherein the lithium solution is LiOH.
16. The method of claim 13, wherein the reducing agent is a green reducing additive. 17 . The method of claim 16 , wherein the green reducing additive is one of ethanol (ET), ethylene glycol (EG) and hydrogen peroxide (HP) or a combination thereof.
18. The method of claim 13, wherein the processing time period is from 2 hours to 20 hours.
19. The method of claim 13, wherein the annealing temperature is in the range of 4000 to 1000°C, and the annealing time period is from 1 hour to 10 hours.
20. The method of claim 19, wherein the annealing temperature is 850°C and the annealing time period is four hours.
21. The method according to claim 13, wherein the NCM powder is LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111).
22. The method according to claim 13, wherein the NCM powder is LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622).
23. The method of claim 13, wherein the aqueous lithium solution is 0.1 M to 4 M LiOH with 1% (v / v) - 3% (v / v) of the reducing agent.