Recycling and reprocessing method of thermoplastic nylon reinforced polyurethane composite material
Through physical separation and chemical purification, low-temperature melting regeneration and the use of functional additives, the problem of recycling TPU composite materials has been solved, and the improvement of material performance and environmentally friendly and efficient recycling have been achieved.
Patent Information
- Application Number
- CN202410888857.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
Existing recycling technology for thermoplastic nylon reinforced polyurethane (TPU) composite materials is difficult to restore the original properties of the material, and the chemical recycling process is complex and costly. It has not been commercially applied on a large scale, and traditional methods are difficult to effectively separate and reprocess.
It adopts physical separation, chemical purification, low-temperature melt regeneration and composite molding methods to separate fibers and matrix through specific chemical solvents, ultrasonic cleaning and heat treatment to purify materials, low-temperature melt regeneration and precise control of blending steps, adding functional additives to enhance Material properties.
It significantly improves the performance of waste TPU composite materials, achieves efficient recycling and reprocessing of materials, reduces production costs, promotes environmentally sustainable development, and avoids environmental pollution caused by traditional recycling methods.
Smart Images

Figure CN118752655A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling and reprocessing of thermoplastic composite materials, in particular to a recycling and reprocessing method for thermoplastic nylon reinforced polyurethane (TPU) composite materials. Background Art
[0002] In modern industrial production, thermoplastic nylon reinforced polyurethane (TPU) composites are widely used in many fields such as automobiles, electronics, aviation, and especially engineering machinery due to their excellent mechanical properties, chemical corrosion resistance and processing convenience. However, with the end of the product life cycle, a large amount of waste TPU composites need to be properly handled. Existing recycling technologies mainly include physical recycling and energy recovery. Physical recycling usually involves steps such as crushing and melt recycling, but these methods often find it difficult to restore the original properties of the material, limiting its high-value reuse. Energy recovery is to recover heat energy by incinerating waste materials, but this method not only wastes the potential value of the material, but may also cause secondary pollution to the environment.
[0003] Chemical recycling is an emerging recycling method that converts waste materials into monomers or oligomers through chemical decomposition, providing new possibilities for the recycling of materials. However, the chemical recycling process is complex, costly, and has strict requirements on equipment and technology, and has not yet been commercialized on a large scale. In addition, the thermosetting characteristics of TPU composites make it difficult to effectively separate and reprocess them through conventional methods, and it is urgent to develop new recycling technologies to solve these problems.
[0004] In view of the shortcomings of the prior art, the present invention proposes an innovative recycling and reprocessing method for thermoplastic nylon reinforced polyurethane composite materials. The method aims to achieve high-efficiency recycling and reprocessing of waste TPU composite materials through a series of optimized steps, including physical separation, chemical purification, low-temperature melt regeneration, composite molding and performance optimization, while maintaining or improving the performance of the material to meet the high standards of industrial applications. Summary of the invention
[0005] The technical solution of the present invention is a recycling and reprocessing method for thermoplastic nylon reinforced polyurethane (TPU) composite materials, aiming to improve the recycling rate of waste TPU composite materials and restore their performance.
[0006] A method for recycling and reprocessing a thermoplastic nylon reinforced polyurethane composite material comprises the following steps:
[0007] 1. Separation step: First, the waste TPU composite material is initially crushed and then soaked in a specific chemical solvent to separate the nylon reinforcing fiber from the polyurethane matrix. The choice of chemical solvent is based on its solubility difference in nylon and polyurethane to ensure effective separation of the matrix without damaging the fiber. The specific details are as follows:
[0008] 101. Pretreatment of waste materials: Collect waste TPU composite materials, reduce their size, and use industrial cutting machines to cut them into small pieces suitable for chemical treatment, with the size controlled within the range of 50mm×50mm×5mm.
[0009] 102.Choice of chemical solvent: Based on the difference in chemical properties between nylon and polyurethane, a chemical solvent is selected that has good solubility for polyurethane and little effect on nylon. For example, dimethylformamide (DMF) or dimethyl sulfoxide (DMSO) is selected as the chemical solvent.
[0010] 103. Soaking process: Place the pretreated TPU pieces into the chemical solvent, control the temperature at 50-60℃ in a constant temperature water bath, and set the soaking time to 2-4 hours to ensure that the polyurethane matrix is fully dissolved while the nylon reinforcing fibers remain intact.
[0011] 104. Separation operation: The soaked material is filtered using a screen to separate the dissolved polyurethane matrix solution from the undissolved nylon fibers. An industrial centrifuge is used to further separate the residual chemical solvent and fibers.
[0012] 105. Recovery of chemical solvents: Chemical solvents containing polyurethane are recovered through distillation towers. The recovered solvents can be recycled to reduce the consumption of raw materials.
[0013] 106. Fiber cleaning: Use deionized water to rinse the separated nylon fibers multiple times to remove the attached chemical solvents and dissolved polyurethane residues to ensure the cleanliness of the fibers.
[0014] 107. Drying treatment: Dry the cleaned nylon fiber in a ventilated environment, or use a hot air circulation drying oven to dry it at 70°C for 2 hours to remove moisture and prepare for the next purification treatment.
[0015] Through the above separation steps, we can effectively separate nylon reinforcement fibers and polyurethane matrix from waste TPU composite materials, providing high-quality raw materials for subsequent regeneration and reprocessing steps. This step is the basis of the entire recycling and reprocessing technology solution, ensuring the smooth progress of subsequent steps and the performance of the final product.
[0016] 2. Purification step: The separated nylon reinforced fibers are further cleaned by ultrasonic cleaning to remove the residual polyurethane matrix and impurities on the surface. The frequency, power and time of ultrasonic cleaning are precisely controlled to optimize the cleaning effect. At the same time, the polyurethane matrix is heat-treated under an inert gas atmosphere to remove components with poor thermal stability and restore its original viscosity. The specific requirements and steps are as follows:
[0017] 201. Ultrasonic cleaning of nylon reinforced fibers: Place the separated nylon reinforced fibers in an ultrasonic cleaning tank and use deionized water as the cleaning medium. Set the ultrasonic frequency to 40kHz, which is an effective frequency for removing tiny particles and deep impurities. Adjust the ultrasonic power to 500W to ensure that there is enough energy for cleaning while avoiding excessive damage to the fibers. Control the cleaning time to 30 minutes to ensure that the polyurethane matrix and impurities remaining on the fiber surface are fully cleaned.
[0018] 202. Optimization of ultrasonic cleaning: During ultrasonic cleaning, the fiber should be stirred regularly to ensure adequate contact between the cleaning liquid and the fiber. A small amount of neutral detergent can be added in due course during the cleaning process to improve cleaning efficiency.
[0019] 203. Post-cleaning treatment: After cleaning, the fibers are separated from the cleaning solution using an industrial filtration system. The remaining moisture and impurities on the fibers are further removed by a centrifuge.
[0020] 204. Heat treatment of polyurethane matrix: The separated and recovered polyurethane matrix is placed in a vacuum oven and heat treated in an atmosphere of inert gas (such as nitrogen or argon). The heat treatment temperature is set at 80°C and the time is controlled at 60 minutes to remove low molecular volatiles and thermally unstable components in the polyurethane.
[0021] 205. Inert gas protection: During the entire heat treatment process, maintain a continuous flow of inert gas to prevent oxidation or degradation of the polyurethane matrix.
[0022] 206. Cooling and collection of the substrate: After the heat treatment is completed, the polyurethane substrate is cooled to room temperature in a controlled cooling environment. The treated polyurethane substrate is collected and prepared for the next step of regeneration.
[0023] 207. Evaluation of purification effect: Performance tests are conducted on nylon fibers after ultrasonic cleaning and polyurethane matrix after heat treatment to evaluate the purification effect. The tests include indicators such as the tensile strength of the fibers and the viscosity of the matrix to ensure that the material performance meets the expected regeneration requirements.
[0024] Through the above purification steps, the nylon reinforcement fiber and the polyurethane matrix are effectively purified, providing high-quality raw materials for the next step of regeneration and composite reprocessing. This step is crucial to ensure the performance of the final product, and also reflects the precise control and optimization of details in the material recycling and reprocessing process of the present invention.
[0025] 3. Regeneration step: The purified nylon reinforcement fiber and polyurethane matrix are regenerated by low-temperature melting. During the regeneration process, the temperature is controlled within a specific range below the melting point of the material to prevent thermal degradation of the material properties. The specific steps and requirements are as follows:
[0026] 301. Regeneration of nylon reinforced fiber: Keep the purified nylon reinforced fiber in a dry environment to ensure that its moisture content is less than 0.5% to avoid bubbles or explosions caused by moisture during the melting process. Use a single screw extruder to regenerate the nylon fiber at a low temperature by melting, and set the melting temperature to be 10-15°C below the melting point of the nylon material. For example, if the melting point of nylon 6 is 220°C, the regeneration temperature is set to 205-210°C.
[0027] 302. Regeneration of polyurethane matrix: The purified polyurethane matrix is dried to remove any residual moisture and ensure product quality during the regeneration process. The regenerated polyurethane matrix is prepared using a twin-screw extruder, and the melt temperature is set 5-10°C below the melting point of the polyurethane material. For example, if the melting point of polyurethane is 180°C, the regeneration temperature is set to 170-175°C.
[0028] 303. Temperature control: During the entire regeneration process, a precise temperature control system is used to ensure the stability and uniformity of the melting temperature and avoid local overheating that may lead to a decrease in material properties.
[0029] 304. Monitoring of melting process: Use melt index tester to monitor the flow properties of materials during melting and recycling process to ensure that the processing properties of recycled materials meet the requirements of subsequent processing.
[0030] 305. Filtration of recycled materials: During the regeneration process, a filtration system is set up to remove insoluble impurities that may exist in the molten material to ensure the purity of the recycled material.
[0031] 306. Cooling and molding of recycled materials: The molten recycled nylon and polyurethane materials are cooled by a cooling device and then formed into granules by a pelletizer to facilitate subsequent composite processing.
[0032] 307. Performance testing of recycled materials: Performance testing of recycled nylon reinforcement fibers and polyurethane matrices, including tensile strength, melt viscosity, etc., to ensure that the recycled materials meet specific performance standards.
[0033] 308. Environmental control: During the entire recycling process, keep the production environment clean to avoid the mixing of dust and other pollutants to ensure the high quality of recycled materials.
[0034] Through the above regeneration steps, the present invention ensures that the purified nylon reinforced fiber and polyurethane matrix can be effectively regenerated at a lower temperature, avoiding thermal degradation of material properties that may be caused by high temperature, while ensuring the processing performance and physical properties of the recycled materials, providing high-quality raw materials for the next step of composite reprocessing. This step is a key link in achieving high-value recycling of waste TPU composite materials.
[0035] 4. Composite reprocessing steps: Mix the recycled nylon and polyurethane in a specific weight ratio and melt blend them through a blending extruder to form a new composite material. The temperature, pressure and screw speed during the blending process are precisely adjusted according to the material properties. The specific process and requirements are as follows:
[0036] 401. Preparation of recycled materials: Ensure the dryness and particle size of recycled nylon and polyurethane particles are uniform to facilitate uniform melting and mixing in the compounding extruder.
[0037] 402. Determination of mixing ratio: Determine the weight ratio of recycled nylon and polyurethane according to the performance requirements of the target composite material. For example, in order to obtain good mechanical properties and processing properties, the weight ratio can be selected in the range of 30:70 to 70:30.
[0038] 403. Setting of blending extruder: Select the appropriate blending extruder model and set the melting temperature of the extruder according to the melt viscosity and melting point of nylon and polyurethane. Usually, the temperature is set at the middle value of the melting points of the two materials to ensure sufficient melting and mixing.
[0039] 404. Temperature control: During the blending process, an extruder with multiple temperature zones is used, with the temperature of each zone slightly higher than the melting point of recycled nylon and polyurethane to ensure uniform melting and mixing of the materials.
[0040] 405. Pressure regulation: According to the melting state and flow behavior of the material, adjust the pressure of the extruder to ensure the continuity and uniformity of the material during the extrusion process.
[0041] 406. Optimization of screw speed: Adjust the screw speed to achieve the best mixing effect and production efficiency. The screw speed is usually optimized based on the melt viscosity of the material and the design of the extruder.
[0042] 407. Monitoring of the Blending Process: Using online sensors and visual inspection systems to monitor the blending process to ensure the quality and consistency of the composite material.
[0043] 408. Material conveying and molding: The blended molten material is passed through the extruder head die and molded into plates, films, fibers or other shapes as required.
[0044] 409. Cooling and solidification: The molded composite material is cooled by a cooling device to solidify the shape and structure of the material.
[0045] 410. Post-processing: The formed composite material is subjected to necessary post-processing, such as cutting, grinding or heat treatment, to meet specific application requirements.
[0046] 411. Performance testing: The blended composite materials are subjected to performance testing, including tensile strength, flexural strength, impact strength, thermal stability, etc., to evaluate the comprehensive performance of the materials.
[0047] Through the above-mentioned composite reprocessing steps, the present invention realizes the effective composite of recycled nylon and polyurethane to form a new composite material with expected performance. This step not only improves the recycling rate of waste materials, but also ensures the high performance and high added value of the composite material by accurately controlling the blending conditions.
[0048] 5. Performance optimization steps: In order to further improve the performance of the composite material, add an appropriate amount of functional additives to the blend, including compatibilizers to improve the compatibility between the fiber and the matrix, stabilizers to improve the thermal stability and light stability of the material, and reinforcing agents to improve the mechanical properties of the material. The specific steps and requirements are as follows:
[0049] 501. Selection of functional additives: According to the expected application and performance requirements of the composite material, select appropriate functional additives. These additives include but are not limited to compatibilizers, stabilizers and reinforcing agents.
[0050] 502. Addition of compatibilizer: Maleic anhydride grafted polyolefin (MAPE) was selected as a compatibilizer to improve the compatibility between nylon fiber and polyurethane matrix. 0.5-2% by weight of MAPE was added to the blend to improve the interfacial adhesion and the mechanical properties of the overall composite material.
[0051] 503. Addition of stabilizers: In order to improve the thermal stability and light stability of the material, a mixture of 0.3-1% by weight of a thermal stabilizer and a light stabilizer is added. Thermal stabilizers such as calcium stearate, and light stabilizers such as ultraviolet absorbers (UVAs) and hindered amine light stabilizers (HALS) are added to prevent thermal and light degradation of the material during processing and use.
[0052] 504. Addition of reinforcing agents: In order to improve the mechanical properties of the material, 1-3% by weight of carbon nanotubes or graphene are added as reinforcing agents. These nanomaterials can provide additional mechanical reinforcement and rigidity while maintaining the lightweight characteristics of the material.
[0053] 505. Dispersion of additives: Use a high-speed mixer or a three-roll mill to evenly disperse the functional additives in the blend to ensure uniform mixing of the additives and the base material.
[0054] 506. Evaluation of dispersion effect: Observe the dispersion of additives in the composite material by scanning electron microscopy (SEM) or transmission electron microscopy (TEM) to ensure that there is no agglomeration.
[0055] 507. Mixing of composites: During the mixing process, the dispersion effect of the additives and the uniformity of the composite material can be optimized by adjusting the mixing time and stirring speed.
[0056] 508. Processing of mixed materials: The composite material with added functional additives is further processed at a suitable temperature, such as extrusion, injection molding or compression molding.
[0057] 509. Performance testing: A series of performance tests are conducted on composite materials with functional additives, including tensile strength, impact strength, heat deformation temperature, weather resistance, etc., to verify the optimization effect of the additives.
[0058] 510. Environmental adaptability assessment: Conduct environmental adaptability assessment on composite materials, such as wet heat aging test, salt spray test, etc., to ensure the stability and reliability of the materials in different environments.
[0059] Through the above performance optimization steps, the present invention not only improves the comprehensive performance of the composite material, but also ensures the stability and durability of the material in various application environments, meeting the strict requirements of the high-performance composite material market.
[0060] The molding process, according to the product design and technical requirements, selects a suitable molding process, such as extrusion, injection molding or compression molding. In extrusion molding, the optimized composite material is pushed by a screw and continuously extruded through a mold of a specific shape to form products such as plates, pipes or rods. In injection molding, after the material is heated and melted, it is injected into a closed mold by high pressure, and demolded after cooling and solidification to obtain the desired three-dimensional shape product. In compression molding, the material is placed in the mold and solidified by pressure and appropriate temperature, which is suitable for manufacturing products with complex shapes such as automotive parts and electronic equipment housings. In the molding process, it is crucial to accurately control the equipment parameters. This includes but is not limited to melting temperature, mold temperature, injection pressure, holding time, cooling rate, etc. For example, in injection molding, the melting temperature needs to be set according to the specific composition and properties of the composite material to ensure that the material is fully melted without degradation; the mold temperature affects the appearance and internal structure of the product and needs to be adjusted according to the product requirements; the control of injection pressure and holding time ensures that the material is fully filled in the mold and reduces the generation of bubbles. In addition, the cooling rate directly affects the dimensional stability and mechanical properties of the product, and must be strictly controlled to avoid shrinkage and deformation after molding. By precisely controlling these parameters, we can ensure that the quality and performance of the molded products meet the design requirements. The molded products also need to undergo necessary post-processing, such as deburring and annealing, to further improve the product's appearance quality and performance. Finally, the molded products will undergo strict quality testing, including dimensional accuracy, mechanical property testing and durability evaluation, to ensure that they meet industry standards and customer requirements.
[0061] The performance test is carried out after the molding process is completed, and a series of comprehensive performance tests are carried out to verify whether the product meets the performance standards of industrial applications. The test process first includes a tensile strength test, in which the sample is stretched until it breaks by a universal material testing machine, and the maximum load and elongation at break are recorded, and the tensile strength and elongation of the material are calculated. Then, an impact strength test is carried out, and a simply supported beam impact testing machine is used to impact the sample to determine its ability to withstand impact force and obtain the impact strength value. The chemical corrosion resistance test is carried out by immersing the sample in specific chemical substances, such as acid, alkali or organic solvent, taking it out after a certain period of time, and evaluating the chemical corrosion resistance of the material by the weight loss rate. In addition, a temperature resistance test is carried out, in which the sample is placed in a high temperature or low temperature environment, and its performance changes at extreme temperatures, such as dimensional stability and mechanical properties, are observed to evaluate the temperature resistance of the material.
[0062] It also includes thermal stability testing, using thermogravimetric analysis (TGA) to evaluate the mass loss of the material during the heating process and determine its thermal decomposition temperature. At the same time, a hardness test is performed, using a Shore hardness tester to measure the hardness value of the material. For transparent or translucent products, transmittance and haze tests are also required to evaluate their optical properties. Finally, a comparative analysis is conducted based on the test results and the performance requirements of industrial applications to ensure that the molded products meet or exceed the preset standards in terms of mechanical properties, chemical resistance, temperature resistance and optical properties. All tests are conducted in accordance with international standards or industry specifications to ensure the accuracy and reliability of the test results. Through these rigorous performance tests, the quality and reliability of the products are ensured, providing a solid quality assurance for the market launch and application of the products.
[0063] The innovation of this technical solution lies in its low-temperature melting regeneration technology, which effectively avoids the thermal degradation of material performance; the purification steps of ultrasonic cleaning and heat treatment completely remove impurities and aging layers on the surface of the material; and through the precisely controlled composite reprocessing steps and performance optimization steps, the high-value reuse of waste TPU composite materials is achieved. These innovative points correspond to each claim in the claims, ensuring the novelty, creativity and practicality of the technology.
[0064] By adopting the above technical solution, the following three technical effects are particularly significant:
[0065] 1. Significantly improve material performance: This technical solution uses low-temperature melt regeneration technology to ensure that the microstructure and macroscopic properties of nylon reinforced fibers and polyurethane matrix are not damaged during the regeneration process. The purification steps of ultrasonic cleaning and heat treatment further remove impurities and aging layers on the surface of the material and restore the original performance of the material. In addition, through the precisely controlled composite reprocessing steps and performance optimization steps, the customization of material performance is achieved, so that the regenerated TPU composite material reaches or even exceeds the performance standards of the original material in terms of tensile strength, impact strength, chemical corrosion resistance and temperature resistance.
[0066] 2. Significantly reduce production costs: The optimized recycling and reprocessing process not only reduces energy consumption and raw material usage, but also avoids environmental disposal costs for waste materials. The recycling of chemical solvents and the efficient operation of ultrasonic cleaning equipment reduce cleaning costs. The inert gas protection used in the heat treatment process reduces the oxidation loss of materials. Melt blending through a blending extruder reduces energy consumption and material waste in the production process. In addition, by adding a small amount of functional additives, the material performance is maximized, reducing dependence on expensive raw materials, thereby significantly reducing production costs.
[0067] 3. Promote environmental sustainable development: The implementation of this technical solution avoids the environmental pollution that may be caused by the traditional methods of treating waste TPU composite materials such as incineration, and realizes the green recycling and reuse of materials. Low-temperature melt regeneration technology reduces carbon emissions in the production process, and the purification steps of ultrasonic cleaning and heat treatment reduce the use and emission of harmful chemicals. By adding environmentally friendly functional additives, the impact of materials on the environment during production and use is further reduced. In addition, the widespread use of recycled materials reduces the demand for virgin materials, helps save resources and protect the ecological environment, and promotes environmental sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 This is a flow chart of the recycling and reprocessing method of the present invention
[0069] Figure 2 Schematic diagram of the separation steps of the present invention
[0070] Figure 3 Schematic diagram of the purification steps of the present invention
[0071] Figure 4 Schematic diagram of the regeneration steps of the present invention
[0072] Figure 5 Schematic diagram of the composite reprocessing steps of the present invention
[0073] Figure 6 Schematic diagram of the performance optimization steps of the present invention DETAILED DESCRIPTION
[0074] Combination Figures 1 to 6 A method for recycling and reprocessing a thermoplastic nylon reinforced polyurethane composite material. To demonstrate the technical solution of the present invention, a detailed embodiment is provided below, including specific parameters and expected results.
[0075] 1. Separation steps:
[0076] The waste TPU composite material was crushed into particles with an average particle size of 5 mm.
[0077] N-methylpyrrolidone was used as a chemical solvent to soak the crushed particles for 24 hours to separate the nylon reinforcing fibers from the polyurethane matrix.
[0078] Mechanical stirring was used at 200 rpm to facilitate the separation process.
[0079] 2. Purification steps:
[0080] The separated nylon reinforced fibers were cleaned in an ultrasonic cleaning device at a frequency of 40 kHz and a power of 300 W for 15 minutes, and the temperature of the cleaning solution was controlled at 50°C.
[0081] The polyurethane matrix was heat treated in a hot air circulation oven at 100 °C for 30 min to remove components with poor thermal stability.
[0082] 3. Regeneration steps:
[0083] The purified nylon reinforcing fibers and polyurethane matrix are melt-regenerated at a temperature 15°C lower than their melting points. For example, if the melting point of nylon is 220°C, the regeneration temperature is controlled at 205°C.
[0084] The twin-screw extruder was used to prepare recycled nylon and recycled polyurethane pellets.
[0085] 4. Composite reprocessing steps:
[0086] Recycled nylon and recycled polyurethane were mixed in a weight ratio of 1:3, and composite pellets were prepared using a blending extruder.
[0087] During the blending process, the melt temperature of the extruder was controlled at 210-230°C and the screw speed was 100 rpm.
[0088] 5.Performance optimization steps:
[0089] 0.5 weight percent of maleic anhydride grafted polyolefin as a compatibilizer, 1 weight percent of a mixture of a heat stabilizer and a light stabilizer, and 1 weight percent of nano carbon tubes as a reinforcing agent were added to the composite particles.
[0090] Mix in a slow mixer for 5 minutes to ensure even dispersion of the additive.
[0091] Forming process:
[0092] The optimized composite particles were molded into standard test samples using an injection molding machine, with the injection temperature controlled at 240 °C and the injection pressure at 80 MPa.
[0093] Performance Test:
[0094] The tensile strength of the molded samples was tested, and the results showed that the tensile strength reached 40MPa, which was 10% higher than that of the original material.
[0095] The impact strength test showed that the impact strength reached 10kJ / m 2 , 20% higher than the original material.
[0096] In the chemical corrosion resistance test, the mass loss of the sample was less than 1% after being immersed in common organic solvents for 72 hours.
[0097] In the temperature resistance test, the samples were cycled in the temperature range of -40℃ to 100℃ without any cracks or deformation.
[0098] Through the above embodiments, the technical solution of the present invention not only realizes the effective recycling and reprocessing of waste TPU composite materials, but also significantly improves the comprehensive performance of the material through precisely controlled process parameters and performance optimization steps, meeting the high standards required for industrial applications. Specific implementation 2:
[0100] This example further illustrates another specific implementation of the present invention, including detailed parameter settings, operation steps and expected results.
[0101] 1. Separation steps:
[0102] The collected waste TPU composite material is cut into blocks with a size less than 100 mm.
[0103] At 50°C, 80% by mass of dimethyl sulfoxide (DMSO) was used as a chemical solvent to soak the block material for 4 hours to achieve the initial separation of the nylon reinforcing fibers and the polyurethane matrix.
[0104] 2. Purification steps:
[0105] The separated nylon reinforcing fibers were separated by a centrifugal separator and ultrasonically cleaned in deionized water at 60° C. for 20 minutes at an ultrasonic frequency of 40 kHz and an ultrasonic power of 200 W to remove attached polyurethane residues.
[0106] The separated polyurethane matrix was heat-treated by heating in a vacuum oven at 120° C. for 45 minutes to remove low molecular volatiles and thermally unstable components.
[0107] 3. Regeneration steps:
[0108] The purified nylon reinforcing fibers are dried at 220°C to remove moisture, and then melt-extruded at 230°C to form recycled nylon pellets.
[0109] The purified polyurethane matrix was melt-regenerated at 190° C., and recycled polyurethane particles were prepared by a single-screw extruder.
[0110] 4. Composite reprocessing steps:
[0111] Recycled nylon and recycled polyurethane were mixed in a weight ratio of 2:3, and composite particles were prepared using a twin-screw extruder. The melt temperature of the extruder was controlled at 240° C. and the screw speed was 200 rpm.
[0112] 5.Performance optimization steps:
[0113] 1 weight percent of a compatibilizer (such as maleic anhydride grafted polypropylene), 0.8 weight percent of an ultraviolet absorber and 0.7 weight percent of an antioxidant are added to the composite particles to improve the weather resistance and chemical resistance of the material.
[0114] Mix in a high-speed mixer for 10 minutes to ensure that the additives are evenly dispersed in the composite particles.
[0115] Forming process:
[0116] The optimized composite particles were molded into standard test samples using an injection molding machine. The mold temperature was controlled at 80°C, the injection pressure was 90 MPa, and the holding time was set to 10 seconds.
[0117] Performance Test:
[0118] The tensile strength of the molded samples was tested, and the results showed that the tensile strength reached 50MPa, meeting the use requirements of automotive parts.
[0119] The impact strength test showed that the impact strength reached 12kJ / m 2 , applicable to drop test standards.
[0120] In the chemical corrosion resistance test, after immersion in common chemicals such as gasoline and engine oil for 96 hours, the mass loss was controlled within 2%.
[0121] Thermal aging tests were carried out and after aging for 1000 hours at 120°C, the retention rates of the tensile strength and impact strength of the material were above 90% and 85% respectively.
[0122] Through Example 2, the technical solution of the present invention once again proves its effectiveness and superiority in the recycling and reprocessing of waste TPU composite materials, achieves a comprehensive improvement in material performance, and meets a wider range of industrial application needs.
Claims
1. A method for recycling and reprocessing thermoplastic nylon reinforced polyurethane composite material, characterized in that The following steps are involved: a. Separation: Use a combination of chemical solvent immersion and mechanical grinding to physically or chemically separate the nylon reinforcing fibers and polyurethane matrix in waste composite materials; b. Purification: The separated nylon reinforced fibers are ultrasonically cleaned, the cleaning liquid temperature is controlled at 40-60°C, and the cleaning time is controlled at 10-30 minutes to remove surface impurities; the polyurethane matrix is heat treated, the temperature is controlled at 80-120°C, and the time is controlled at 15-45 minutes to remove the aging layer; c. Regeneration: Using low-temperature melting technology, the purified nylon reinforcement fiber and polyurethane matrix are melted and regenerated at a temperature 10-20°C below their melting point to avoid thermal degradation of material properties; d. Composite reprocessing: According to the performance requirements of the required composite material, the recycled nylon and recycled polyurethane are mixed in a weight ratio of 1:1 to 1:4, and composite molding is performed under specific temperature and pressure conditions to form a new thermoplastic nylon reinforced polyurethane composite material; e. Performance optimization: Add 0.5-2% by weight of functional additives, including compatibilizers, stabilizers and reinforcing agents, to the composite reprocessed materials to improve the compatibility, stability and mechanical properties of the materials.
2. The method according to claim 1, characterized in that The chemical solvent is an environmentally friendly solvent that has good solubility for both nylon and polyurethane, such as N-methylpyrrolidone or dimethyl sulfoxide.
3. The method according to claim 1 or 2, characterized in that: The ultrasonic frequency used in the ultrasonic cleaning process is 40kHz and the ultrasonic power is 100-500W.
4. The method according to claim 1, characterized in that: Inert gas protection is used during the heat treatment process to prevent oxidation of the polyurethane matrix.
5. The method according to claim 1, characterized in that The equipment used in low temperature melting technology enables precise temperature control and uniform melting results.
6. The method according to claim 1, characterized in that The reactor used in the compounding reprocessing step has an adjustable temperature and pressure control system to accommodate the compounding requirements of different materials.
7. The method according to claim 1, characterized in that The compatibilizer added in the performance optimization step is maleic anhydride grafted polyolefin, the stabilizer is a mixture of a heat stabilizer and a light stabilizer, and the reinforcing agent is nano-scale carbon tubes or graphene.
8. A thermoplastic nylon reinforced polyurethane composite material obtained by the method according to any one of claims 1 to 7, characterized in that: The material has higher tensile strength and impact strength than the original material, as well as better chemical corrosion resistance and temperature resistance.
9. The composite material according to claim 8, characterized in that The material is suitable for manufacturing automotive parts, electronic equipment housings, aviation components or sporting goods with high performance requirements.
10. A device using the method according to any one of claims 1 to 9, characterized in that: It includes units for separation, purification, regeneration and composite reprocessing, as well as control systems for precise control of temperature, pressure and additive addition to ensure the efficiency and stability of the material recycling and reprocessing process.
Citation Information
Patent Citations
Method for the pretreatment, reprocessing or recycling of thermoplastic material
CN101535018A
Separation method for polyurethane and nylon mixed powder and application of separation method
CN105058620A
Mechanical recycling of multicomponent polymeric waste comprising polyamide and polyurethane
WO2023199251A1