Titanium-based phosphate active material as well as preparation method and application thereof
By combining the solid-state reaction high-temperature sintering process and using industrial pure raw materials to prepare titanium-based phosphate battery materials, the problem of the impact of impurities in the preparation of industrial pure raw materials is solved, the efficient preparation of materials and the improvement of electrochemical performance are achieved, and the cost and crystal are reduced. defect.
Patent Information
- Application Number
- CN202410736770.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
It is difficult to effectively utilize industrial pure raw materials to prepare titanium-based phosphate battery materials using existing technology, and the electrochemical properties of the materials are affected by impurity elements, resulting in high costs and unstable performance.
Titanium-based phosphate powder is prepared by using low-quality industrial pure raw materials combined with solid-state reaction and high-temperature sintering. By selecting appropriate treatment agents and processes, electrode active materials with good electrochemical properties are prepared. Specific steps include dissolving the precursor raw material in a solvent, dispersing it, reacting with reagents, precipitating and wet grinding, spray drying and sintering, and finally obtaining a titanium-based phosphate active material with D50<1 μm.
It reduces the quality control purity requirements of raw materials, improves the synthesis purity and electrochemical performance of materials, reduces preparation costs, and promotes the improvement of grain morphology and size distribution through the action of hydroxide ions and divalent alkali metal cations. Uniformity, reducing crystal defects and enhancing battery performance.
Smart Images

Figure CN118754076A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a titanium-based phosphate active material and a preparation method and application thereof, belonging to the technical field of batteries. Background Art
[0002] There are many methods for synthesizing polyanionic phosphate materials in the industry, and conventional synthesis methods also include solid-phase reaction and sol-gel preparation methods. However, there are few reports on controlling the synthesis of polyanionic materials by adapting the specifications of raw materials. That is, most of the current methods are laboratory synthesized, which only adds relevant elements as reaction precursors based on the theoretical synthesis chemical reaction equation of sodium titanium phosphate, but it is difficult to directly apply it to the actual industrial production process. This is because industrial pure raw materials contain impurities, which account for about 1.5-3%, and the impurity elements of the raw materials have a direct impact on the performance of the target product of the final synthesis. Moreover, there is a direct correlation between the cost and purity of raw materials. Therefore, how to find a process route suitable for the preparation of titanium-based phosphate powders with industrial pure raw materials is of great significance to the cost reduction and efficiency improvement of enterprises. Summary of the invention
[0003] To solve the above problems, the present invention provides a method for preparing titanium-based phosphate powder by combining low-quality industrial pure raw materials with solid phase reaction and high-temperature sintering. According to the characteristics of the industrial-grade raw materials, a suitable treating agent is selected for treatment to prepare an electrode active material that can meet the electrochemical properties of titanium-based phosphate as a sodium ion battery material.
[0004] The first object of the present invention is to provide a method for preparing a titanium-based phosphate active material, comprising the following steps:
[0005] S1, dissolving a precursor raw material in a solvent and dispersing it with a dispersant to obtain a mixed solution; the precursor raw material includes a soluble sodium source, a soluble phosphorus source and an organic carbon source;
[0006] S2, reacting the mixed solution of step S1 with reagent 1 and reagent 2, and separating the precipitate and the solution after the reaction is completed;
[0007] S3, performing air flow pulverization on the titanium source with D50=10-20 μm to make it D50=1-5 μm, mixing the pulverized titanium source with the solution separated in step S2 and the inorganic carbon source to obtain a mixed slurry, and wet grinding the mixed slurry to reduce the particle size of the mixed slurry to D50<1 μm to obtain a precursor slurry;
[0008] S4, spray drying the precursor slurry in step S3 to obtain a precursor powder;
[0009] S5, sintering the precursor powder of step S4 under an inert atmosphere;
[0010] S6, performing air flow crushing on the product sintered in step S5 to remove magnetism, thereby obtaining the titanium-based phosphate active material;
[0011] The sodium source and phosphorus source are industrial pure raw materials (purity is 70-99.5%, which can be selected according to actual industrial raw materials), and the purity of the titanium source is >99%;
[0012] The reagent 1 is selected from sodium hydroxide or ammonia water, and the reagent 2 is selected from one or more of barium carbonate, barium chloride, calcium chloride and calcium hydroxide.
[0013] Preferably, the molar ratio of the reagent 1 to the sodium source is (0.02-0.1):1, and the molar ratio of the reagent 2 to the sodium source is (0.02-0.1):1.
[0014] Furthermore, the concentration of the aqueous ammonia is 20-30%, preferably 25-28%.
[0015] Furthermore, the purity of the industrial pure raw material is 70-99.5%, such as 70%, 73%, 75%, 77%, 80%, 85%, 88%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, etc., including but not limited to the purity values listed above.
[0016] Furthermore, in step S1, the sodium source is one or more soluble sodium salts. Preferably, the sodium source is sodium carbonate (soda ash), industrial pure-98%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%; sodium phosphate (sodium phosphate), industrial pure-98%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%.
[0017] Further, in step S1, the phosphorus source is one or more soluble phosphorus-containing acids or salts, preferably monoammonium phosphate (MAP) or diammonium phosphate (DAP), industrial pure-98%, industrial pure-98.5%, industrial pure-99%; orthophosphoric acid, industrial pure-85%, industrial pure-90%, industrial pure-95%; metaphosphoric acid or phosphoric acid, industrial pure-70%, industrial pure-80%, industrial pure-95%; or sodium pyrophosphate, industrial pure-96%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%.
[0018] Further, in step S1, the organic carbon source is selected from one or more of glucose, sucrose, polyvinyl alcohol compounds (PEG), citric acid, and polyacrylic acid compounds. The molar ratio of the organic carbon source to the sodium source is (0.01-0.5):1, such as 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, etc.
[0019] Furthermore, in step S1, the dispersant is an inorganic alkali metal phosphate compound and / or an organic polymer compound. Inorganic alkali metal phosphate compounds include sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate, etc.; organic polymers include at least one of polyacrylic acid, polyvinyl alcohol and polyethylene glycol. The amount of the dispersant is 0.1-2wt% of the precursor raw material.
[0020] Furthermore, in step S1, the solvent is water, such as ordinary industrial water.
[0021] Furthermore, the molar ratio of the sodium source, phosphorus source and titanium source is 1:3-5:1-2, such as 1:3:1, 1:3.5:1, 1:3.8:1, 1:4:1, 1:5:1, 1:3:1.5, 1:3.5:1.5, 1:3.8:1.5, 1:4:1.5, 1:5:1.5, etc., including but not limited to the ratios listed above.
[0022] Further, in step S3, the titanium source is titanium dioxide, preferably anatase, and the particle size D50 of the titanium dioxide is 10-20 μm, such as 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc., including but not limited to the particle size values listed above.
[0023] Furthermore, in step S3, after air flow pulverization, the particle size D50 of the titanium dioxide is 1-5 μm, such as 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, etc., including but not limited to the particle size values listed above.
[0024] Further, in step S3, the inorganic carbon source is selected from one or more of conductive carbon black, acetylene black, ketjen black, artificial graphite, natural graphite, carbon fiber, carbon nanotube dry powder, graphene, and carbon nanotube aqueous dispersion. The molar ratio of the inorganic carbon source to the sodium source in the precursor is (0.01-0.5):1, such as 0.05:1, 0.1:1, 0.15:1, 0.2:1, 0.25:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, etc.
[0025] Furthermore, in step S3, the wet grinding is performed by using an external circulation ultrafine sand mill with a rotation speed of 300-1000 r / min, the ball milling beads are made of zirconium oxide with a diameter of 0.1-1 mm, the ball milling time is 2-6 hours, and the solid content is 20-60 wt%.
[0026] Furthermore, in step S4, the spray drying is performed at an air inlet temperature of 180-240°C, an air outlet temperature of 90-120°C, and a centrifugal speed of 25000-35000 r / min.
[0027] Further, in step S5, the inert protective atmosphere is provided by an inert gas, such as nitrogen, helium, neon, argon, krypton, xenon, radon, etc., including but not limited to the gases listed above.
[0028] Furthermore, in step S5, in the inert protective atmosphere, the gas flow rate is 10-300 ml / min, and the gas purity is between 99.99-99.999%.
[0029] Further, in step S5, the sintering is to heat the precursor powder to 300-400°C at a heating rate of 1-10°C / min and keep it at a constant temperature for 1-5 hours, first performing pre-sintering and cracking and coating of organic carbon; then further heating to 600-800°C, and calcining at this temperature for 5-10 hours; after sintering is completed, the titanium-based phosphate active material is obtained by natural cooling. During the first stage of calcination, the heating temperature includes but is not limited to 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, and 400°C, and the insulation time includes but is not limited to 1 hour, 2 hours, 3 hours, 4 hours, and 5 hours; during the second stage of calcination, the heating temperature includes but is not limited to 600°C, 620°C, 650°C, 680°C, 700°C, 720°C, 750°C, 770°C, and 800°C, and the insulation time includes but is not limited to 5 hours, 6 hours, 7 hours, 8 hours, and 9 hours.
[0030] The second object of the present invention is to provide an electrode active material obtained by the above preparation method, wherein the structural formula of the electrode active material is Na a Ti b X c , wherein X is a phosphate group, a=1-2, b=1-2, c=3-5, and the values of a, b, c, and d satisfy the charge balance of the chemical formula.
[0031] The third object of the present invention is to provide an electrode plate, comprising an electrode active layer, wherein the electrode active layer comprises the electrode active material, a conductive agent and a binder.
[0032] Furthermore, the electrode active layer comprises the following components in mass percentage: 75-95% of active material, 5-15% of conductive agent and 5-15% of binder.
[0033] Furthermore, the conductive agent is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0034] Furthermore, the binder can be any binder well known to those skilled in the art without any particular limitation, such as one or more of chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer.
[0035] Furthermore, the thickness of the electrode active layer is preferably in the range of 150-250 μm, for example, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, etc., including but not limited to the thickness values listed above.
[0036] A fourth object of the present invention is to provide a method for preparing the electrode sheet as described above, comprising the following steps:
[0037] S01, adding the formulated amount of active material, conductive agent, and binder into water and stirring evenly to obtain active slurry;
[0038] S02, coating the active slurry on at least one side of the current collector along the thickness direction, drying to obtain an active layer, and pressing to obtain the electrode plate.
[0039] Furthermore, the current collector is aluminum foil, or other materials that can be used as a current collector; preferably, the thickness of the current collector is in the range of 4-8 μm.
[0040] Beneficial effects of the present invention:
[0041] The present invention is directed to Na a Ti b X cMaterials, the preparation process is designed starting from industrial-grade raw materials, specifically including industrial-pure sodium source, phosphorus source, and untreated large-particle titanium source, which greatly reduces the quality control purity requirements of raw materials, and through screening of multiple treatment methods, it is found that when an appropriate amount of sodium hydroxide / ammonia water is used in combination with barium carbonate / barium chloride / calcium chloride / calcium hydroxide, it can not only remove the iron ions and sulfate ions that have a greater impact on the electrochemical properties, but also improve the purity of material synthesis. On the other hand, an appropriate excess of treatment reagents will introduce hydroxide ions and divalent alkali metal cations. Hydroxide ions will inhibit the growth behavior of grains and promote the uniformity of grain morphology and size distribution. Trace amounts of divalent alkali metal cations can improve the stability of the powder lattice structure, which can reduce crystal defects and enhance battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 Schematic diagram of the synthesis process of titanium-based phosphate powder.
[0043] Figure 2 This is the microscopic morphology of the powder prepared in Example 1.
[0044] Figure 3 This is the XRD of the powders prepared in Example 1 and Comparative Example 2.
[0045] Figure 4 Photos of liquid impurity removal before and after filtration.
[0046] Figure 5 is the initial particle size of titanium dioxide.
[0047] Figure 6 It is the particle size of titanium dioxide after air flow grinding.
[0048] Figure 7 It is the particle size of mixed slurry after ultrafine grinding.
[0049] Figure 8 The charge capacity and cycle performance of the powder prepared in Example 1. DETAILED DESCRIPTION
[0050] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0051] As described in the background technology, the synthesis cost of titanium-based phosphate, a polyanion material in aqueous sodium-ion batteries, is currently high. The use of industrial-grade raw materials is of great significance for large-scale industrial production. However, impurities in industrial-grade raw materials have an impact on the performance of the final prepared battery. Currently, no one has studied what specific factors affect the performance and how to solve this problem.
[0052] The present invention provides a method for preparing a titanium-based phosphate active material for a battery, comprising the following steps:
[0053] S1, dissolving a precursor raw material in water and dispersing it with a dispersant to obtain a mixed solution; the precursor raw material includes a sodium source, a phosphorus source and an organic carbon source;
[0054] S2, reacting the mixed solution of step S1 with reagent 1 and reagent 2, and separating the precipitate and the solution after the reaction is completed;
[0055] S3, performing air flow pulverization on the titanium source with D50=10-20 μm to make it D50=1-5 μm, mixing the pulverized titanium source with the solution separated in step S2 and the inorganic carbon source to obtain a mixed slurry, and wet grinding the mixed slurry to reduce the particle size of the mixed slurry to D50<1 μm to obtain a precursor slurry;
[0056] S4, spray drying the precursor slurry in step S3 to obtain a precursor powder;
[0057] S5, sintering the precursor powder of step S4 under an inert protective atmosphere;
[0058] S6, performing air flow crushing on the product sintered in step S5 to remove magnetism, thereby obtaining the titanium-based phosphate active material;
[0059] The sodium source and phosphorus source are industrial pure (purity is 70-99.5%), and the purity of the titanium source is >99%;
[0060] The reagent 1 is selected from sodium hydroxide or ammonia water, and the reagent 2 is selected from one or more of barium carbonate, barium chloride, calcium chloride and calcium hydroxide.
[0061] The molar ratio of the reagent 1 to the sodium source is (0.02-0.1):1, and the molar ratio of the reagent 2 to the sodium source is (0.02-0.1):1.
[0062] In the present invention, industrial-grade chemical reagents are used as raw materials, which can greatly reduce the preparation cost of materials; for the preparation of phosphate materials of specific composition, we select reagents 1 and 2 to process industrial-grade raw materials, which can remove iron ions and sulfate ions that have a greater impact on electrochemical performance and improve the purity of material synthesis; on the other hand, we found that appropriate excess of reagents 1 and 2 will introduce hydroxide ions and divalent alkali metal cations, and hydroxide ions will inhibit the growth behavior of grains and promote the uniformity of grain morphology and size distribution. Trace divalent alkali metal cations have an improving effect on the stability of the powder lattice structure, which can reduce crystal defects and enhance battery performance.
[0063] Preferably, the steps are as follows:
[0064] S1. Preparation of mixed slurry of precursors: Sodium source, phosphorus source and organic carbon source are dissolved in a certain amount of deionized water, dispersant is added, stirred and dissolved completely, then reagents 1 and 2 are added, stirring is continued, and after the precipitation reaction is fully completed for a period of time, the precipitation impurities are removed by filter pressing. At the same time, the titanium dioxide raw materials are initially crushed by air flow milling to reduce the particle size. The filtered clarified liquid is continued to be added with the inorganic carbon source and the treated titanium dioxide powder, and the slurry is prepared by wet ultrafine grinding and mixing, and the slurry is ground evenly and set aside.
[0065] S2, precursor spray drying granulation preparation: the precursor slurry obtained in step S1 is spray dried to remove the solvent, and the secondary particle size and coating morphology of the precursor mixed powder agglomerate are controlled by controlling the spray drying inlet air temperature, centrifugal speed, feed speed, etc.;
[0066] S3. Synthesis and preparation of polyanion materials: The precursor powder obtained in step S2 is loaded into a graphite sagger, and then placed into a kiln for sintering according to a set sintering process curve. During the sintering process, an inert gas is used for protection throughout the process.
[0067] S4. After the sintered materials are collected, they are air flow crushed and sieved for demagnetization. The obtained powders are collected and packaged for storage for later use. After the powders are dried and dehumidified, they are further slurried and coated, and assembled with buttons for powder performance characterization tests.
[0068] As mentioned above, industrial pure raw materials contain a variety of impurities, but due to the lack of relevant research, it is not clear what elements are beneficial to the electrochemical performance of titanium-based phosphate materials, and what impurities are harmful to them, and there is a lack of research on the preparation process starting from industrial-grade raw materials. Therefore, after a large number of screenings and careful designs, the present invention finds that when two reagents are used in combination and a certain ratio is maintained, the obtained phosphate material has good electrochemical properties. The preparation method can effectively reduce the cost of polyanion materials, reduce the crystal defects of materials, etc.
[0069] The sodium source is one or more soluble sodium salts. For example, sodium carbonate, sodium phosphate, sodium oxalate, sodium acetate, sodium formate, sodium citrate, etc., including but not limited to the sodium sources listed above. Preferably, the sodium source is sodium carbonate (soda ash), industrial pure-98%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%; sodium phosphate (sodium phosphate), industrial pure-98%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%.
[0070] The phosphorus source is monoammonium phosphate (MAP) or diammonium phosphate (DAP), industrial pure-98%, industrial pure-98.5%, industrial pure-99%; orthophosphoric acid, industrial pure-85%, industrial pure-90%, industrial pure-95%; metaphosphoric acid or phosphoric acid, industrial pure-70%, industrial pure-80%, industrial pure-95%; or sodium pyrophosphate, industrial pure-96%, industrial pure-98.5%, industrial pure-99%, industrial pure-99.5%.
[0071] The organic carbon source is selected from one or more of glucose, sucrose, polyvinyl alcohol compounds (PEG), citric acid, and polyacrylic acid compounds. The molar ratio of the organic carbon source to the sodium source is (0.01-0.5):1.
[0072] The dispersant is an inorganic alkali metal phosphate compound and / or an organic polymer compound. Inorganic alkali metal phosphate compounds include sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate; organic polymers include at least one of polyacrylic acid, polyvinyl alcohol and polyethylene glycol. The amount of the dispersant is 0.1-2wt% of the precursor raw material.
[0073] Preferably, the molar ratio of the sodium source, the phosphorus source and the titanium source is 1:3-5:1-2, and a titanium-based phosphate battery material of a specific composition is prepared in this ratio, and reagent one and reagent two are combined to obtain a structurally stable material.
[0074] In step S3, the titanium source is titanium dioxide, preferably anatase, and the particle size D50 of the titanium dioxide is 10-20 μm. For example, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, etc., including but not limited to the particle size values listed above. Among the three key raw materials for synthesizing sodium titanium phosphate, titanium dioxide is the core of the solid phase reaction, and the selection of the titanium source is particularly important. For example, the particle size grade of titanium dioxide directly determines the price compared to the purity grade. The smaller the particle size, the higher the price, and the larger the particle size, the lower the price. The present invention targets titanium dioxide with large particle size and performs nano-processing on titanium dioxide, which can effectively reduce the energy consumption of the reaction process and improve the crystal purity of the material. At the same time, it controls the synthetic particle size of the titanium-based phosphate powder, making the coating effect of the carbon material more sufficient, improving the conductivity of the powder and reducing the ion diffusion path, so that the prepared titanium-based phosphate has excellent electrochemical properties.
[0075] After air flow pulverization, the particle size D50 of titanium dioxide is 1-5μm; after wet grinding, the particle size D50 of titanium dioxide is <1μm. The present invention adopts a wet step-by-step ball milling method. According to the characteristics of the raw materials, for the soluble sodium source and phosphorus source, a precipitation filtration method is adopted to remove impurity elements. For titanium dioxide as a titanium source, the cost of the raw materials is directly related to the particle size. The air flow pulverization method is used in advance to effectively reduce the initial particle size of the powder. Combined with ultrafine grinding to prepare a mixed slurry, the uniformity of the slurry and the microscopic control of the powder morphology can be significantly improved, which lays a good foundation for the solid-phase reaction process of sintering and crystal production. The entire process operation process has low environmental requirements, greatly reduces the specification and quality control of raw materials, effectively reduces costs, and can be produced continuously, with high industrial application value.
[0076] The inorganic carbon source is selected from one or more of conductive carbon black, acetylene black, Ketjen black, artificial graphite, natural graphite, carbon fiber, carbon nanotube dry powder, graphene, and carbon nanotube aqueous dispersion. The molar ratio of the inorganic carbon source to the sodium source in the precursor is (0.01-0.5):1.
[0077] When the sodium ion battery is prepared by using the above active material, it contains a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, and the positive electrode or the negative electrode sheet contains the above active material.
[0078] Example 1
[0079] S1, dissolve 20g of polyacrylic acid as a dispersant in 10L of deionized water, stir evenly for 30min, add sodium carbonate (industrial pure-99%, Shanghai Qiren, in compliance with standard GB / T 210.1-2004), diammonium phosphate (industrial pure-99%, Suzhou Dongbai Chemical Co., Ltd., in compliance with standard GB / T 19037-2015), and polyethylene glycol as organic carbon sources, wherein the three powders are weighed in a total mass of 1kg according to a molar ratio of 1:3:0.5, and then add 0.05mol of reagent sodium hydroxide and 0.05mol of reagent barium dicarbonate, continue stirring, wait for the precipitation reaction to be fully completed for a period of time, and then use the form of filter press to complete the removal of precipitated impurities. At the same time, the titanium dioxide raw material (anatase type, purity>99%, D50>10 microns) is initially crushed in the form of air flow milling to reduce the particle size to D50: 2-5 microns. The filtered clarified liquid is continued to be added with 20 g of inorganic carbon source acetylene black and treated titanium dioxide powder, the molar ratio of titanium source to sodium source is 1.95:1, and the slurry is prepared by wet ultrafine grinding and mixing until the mixed slurry particle size D50 is less than 1 micron. Grind evenly and set aside.
[0080] S2, precursor powder drying step: the mixed slurry prepared in S1 is spray dried to remove the solvent, wherein the feed rate is set at 200 ml / min, the air inlet temperature is 230°C, the air outlet temperature is 105°C, and the atomizing disk speed is 25000 r / min. The dried powder is collected and then set aside.
[0081] S3, synthesis and preparation of polyanion materials: the precursor powder obtained in step S2 is loaded into a graphite sagger, and then placed in a kiln for sintering according to a set sintering process curve. During the sintering process, an inert gas is used for protection throughout the process.
[0082] The first step is to start the sintering temperature at room temperature of 20°C, increase the temperature at a rate of 5°C / min, increase the temperature to 350°C and keep it warm for 2 hours; remove the crystalline water and the cracking of the organic carbon source and the tail gas of the solid phase reaction; the second step is to continue to increase the temperature from 350°C at a rate of 3°C / min to 750°C and keep it warm for 10 hours to synthesize the Na1Ti2(PO4)3 phase and grow the grain size;
[0083] S4. After the sintered materials are collected, they are air flow crushed and sieved for demagnetization. The obtained powders are collected and packaged for storage for later use. After the powders are dried and dehumidified, they are further slurried and coated, and assembled with buttons for powder performance characterization tests.
[0084] Example 2
[0085] S1, dissolve 10g of polyvinyl alcohol as a dispersant in 10L of deionized water, stir evenly for 30min, add sodium phosphate (industrial pure-99%), monoammonium phosphate (industrial pure-99%), and sucrose, wherein the three powders are weighed in a molar ratio of 1:3.5:0.2 to a total mass of 1kg, and then add 0.1mol of 25% ammonia water and 0.02mol of barium chloride, continue stirring and wait for the precipitation reaction to be fully completed for a period of time, and then use the form of filter press to complete the removal of precipitated impurities. At the same time, the titanium dioxide raw material (rutile type, purity>99%, D50>10 microns) is initially crushed in the form of air flow milling to reduce the particle size to D50: 2-5 microns. The filtered clarified liquid is continued to add 20g of inorganic carbon source acetylene black and treated titanium dioxide powder, the molar ratio of titanium source to sodium source is 1.5:1, and the slurry is prepared by wet ultrafine grinding and mixing until the mixed slurry particle size D50 is less than 1 micron, and the mixed slurry is ground evenly and then used.
[0086] S2, precursor powder drying step: the mixed slurry prepared in S1 is spray dried to remove the solvent, wherein the feed rate is set at 200 ml / min, the air inlet temperature is 200°C, the air outlet temperature is 120°C, and the atomizing disk speed is 30000 r / min. The dried powder is collected and then used.
[0087] S3, synthesis and preparation of polyanion materials: the precursor powder obtained in step S2 is loaded into a graphite sagger, and then placed in a kiln for sintering according to a set sintering process curve. During the sintering process, an inert gas is used for protection throughout the process.
[0088] The first step is to start the sintering temperature at room temperature of 20°C, increase the temperature at a rate of 6°C / min, increase the temperature to 400°C and keep it warm for 2.5h; remove the crystalline water and the cracking of the organic carbon source and the tail gas of the solid phase reaction; the second step is to continue to increase the temperature from 400°C, increase the temperature at a rate of 5°C / min, increase the temperature to 700°C, keep it warm for 8h, and synthesize the Na1Ti2(PO4)3 phase and grow the grain size;
[0089] S4. After the sintered materials are collected, they are air flow crushed and sieved for demagnetization. The obtained powders are collected and packaged for storage for later use. After the powders are dried and dehumidified, they are further slurried and coated, and assembled with buttons for powder performance characterization tests.
[0090] Example 3
[0091] S1, dissolve 20g of polyacrylic acid as a dispersant in 10L of deionized water, stir evenly for 30min, add phosphoric acid (industrial pure - 95%, Suzhou Dongbai Chemical Co., Ltd., in accordance with the standard GB / T19037-2015), sodium carbonate (purity 98%, Shanghai Qiren, in accordance with the standard GB / T 210.1-2004) and glucose, wherein the three powders are weighed at a molar ratio of 3.8:1:0.5 to a total mass of 1kg, and then add 0.1mol of sodium hydroxide and 0.05mol of calcium hydroxide, continue stirring and wait for the precipitation reaction to be fully completed for a period of time, and then use the form of filter press to complete the removal of precipitated impurities. At the same time, the titanium dioxide raw material (anatase type, purity>99%, D50>10 microns) is initially crushed in the form of air flow milling to reduce the particle size to D50: 1-5 microns. The filtered clarified liquid is continued to be added with 20 g of inorganic carbon source acetylene black and treated titanium dioxide powder, the molar ratio of titanium source to sodium source is 1.2:1, and the slurry is prepared by wet ultrafine grinding and mixing until the mixed slurry particle size D50 is less than 1 micron. Grind evenly and set aside.
[0092] S2, precursor powder drying step: the mixed slurry prepared in S1 is spray dried to remove the solvent, wherein the feed rate is set at 200 ml / min, the air inlet temperature is 180°C, the air outlet temperature is 90°C, and the atomizing disk speed is 35000 r / min. The dried powder is collected and then set aside.
[0093] S3, synthesis and preparation of polyanion materials: the precursor powder obtained in step S2 is loaded into a graphite sagger, and then placed in a kiln for sintering according to a set sintering process curve. During the sintering process, an inert gas is used for protection throughout the process.
[0094] The first step is to start the sintering temperature at room temperature of 20°C, increase the temperature at a rate of 4°C / min, increase the temperature to 300°C and keep it warm for 5 hours; remove the crystalline water and the cracking of the organic carbon source and the tail gas of the solid phase reaction; the second step is to continue to increase the temperature from 300°C, increase the temperature at a rate of 6°C / min, increase the temperature to 800°C, keep it warm for 5 hours, and synthesize the Na1Ti2(PO4)3 phase and grow the grain size;
[0095] S4. After the sintered materials are collected, they are air flow crushed and sieved for demagnetization. The obtained powders are collected and packaged for storage for later use. After the powders are dried and dehumidified, they are further slurried and coated, and assembled with buttons for powder performance characterization tests.
[0096] Comparative Example 1
[0097] The titanium dioxide was not subjected to air flow pulverization, and the remaining steps were the same as those in Example 1.
[0098] Comparative Example 2
[0099] Without adding reagent 1 and reagent 2, the remaining steps are the same as those in Example 1.
[0100] Comparative Example 3
[0101] No reagent 1 was added, and ethylenediaminetetraacetic acid (EDTA) chelating agent was used instead. The remaining steps were the same as in Example 1.
[0102] Comparative Example 4
[0103] Without adding reagent 2, the remaining steps were the same as in Example 1.
[0104] Comparative Example 5
[0105] In order to compare with the preparation process of the present invention using industrial pure raw materials, Na1Ti2(PO4)3 was prepared by solid phase synthesis using high-purity raw materials. The sodium source used was 99.8% sodium carbonate (Shanghai Aladdin Biochemical Technology Co., Ltd.), and the phosphorus source used was 99.9% diammonium phosphate (Shanghai Aladdin Biochemical Technology Co., Ltd.). Reagent 1 and reagent 2 were not added, and the remaining steps were the same as in Example 1.
[0106] Test Case
[0107] Sodium ion batteries were constructed using the titanium-based phosphate active materials prepared in Examples 1-3 and Comparative Examples 1-5, and the electrical properties of each battery were tested.
[0108] (1) Preparation of sodium ion batteries
[0109] The titanium-based phosphate material prepared in Examples 1-3 and Comparative Examples 1-5 was dispersed in NMP with PVDF and acetylene black in a mass ratio of 80:10:10. After being evenly dispersed by ball milling, it was coated on aluminum foil and vacuum dried to obtain a positive electrode. The electrolyte was 1 mol / L NaPF6, in which the solvent volume ratio was EC:DMC:EMC=1:1:1 (volume ratio), the diaphragm was Celgard polypropylene film, and the metal sodium sheet was the negative electrode, which were assembled together into a button half-cell.
[0110] (2) Performance testing
[0111] The test voltage range is 1.5V to 3.5V. It is charged to 3.5V by constant current charging and discharged to 1.5V by constant current discharge. The charge and discharge current is 0.1C. After two cycles of activation, the test is performed at a rate of 1C to confirm the specific capacity of the obtained powder and calculate the capacity retention rate R after 1000 cycles. R = specific capacity after 1000 cycles / initial specific capacity*100%. The test results are shown in Table 1. Figure 8 The charge and discharge curves and cycle performance curves of Example 1 are given in FIG.
[0112] Table 1: Specific capacity and cycle performance of powder charge test of different embodiments and comparative examples
[0113]
[0114]
[0115] The titanium dioxide in Comparative Example 1 was not crushed, and its specific capacity decreased by about 25%. This is mainly because the industrial preparation process of titanium dioxide is mostly sulfuric acid method, the primary particle size of the prepared is nanometer level, and the secondary particle size D50 is 10-20 microns (by Figure 5 It can be seen that after crushing, the secondary particle size D 50 drops to below 5 microns ( Figure 6 ). In comparative example 1, the large particles of titanium dioxide are not conducive to a more complete reaction with the sodium source and the phosphorus source, and the content of the impurities increases accordingly, resulting in a decrease in the specific capacity; at the same time, there is a free phosphorus source that does not participate in the reaction, which acts as a pH corrosion inhibitor during the battery charging and discharging process, triggering hydrogen and oxygen evolution reactions, accelerating the side reactions of the material and the electrolyte, and reducing the capacity retention rate.
[0116] In the preparation process of Comparative Examples 2 and 4, Reagent 1 and / or Reagent 2 are not used, and the specific capacity and cycle performance of the obtained materials are sharply reduced. This may be because one of the contributions of Reagent 1 is to remove Fe ions in the raw materials. The impurity metal content of the industrial-grade raw materials, mainly Fe element, is about 0.5-1%, and the material prepared without adding Reagent 1 has a large amount of impurities in the material synthesis process due to the presence of Fe element, and the iron impurities will interfere with the electrochemical reaction process of the electrode material prepared by the present invention. The iron ions are also easy to react chemically with the electrolyte to produce insoluble precipitates, which accelerates the degradation of the electrolyte, leading to The main contribution of reagent 2 is to remove sulfate impurities in the raw materials through precipitation reaction. Sulfate impurities cannot volatilize during the sintering process. Sulfate may react chemically with certain ions in the electrode material to form insoluble precipitates that block the electrode pores, affecting the ion transport and reaction kinetics of the electrode. It may also react with the electrode material at the interface to generate products that are not conducive to the electrochemical reaction, increase electrode polarization, and lead to a decrease in the specific capacity of the material. During the charge and discharge process, sulfate will undergo electrochemical decomposition reaction to produce gas and other by-products, affecting the cycle performance of the battery.
[0117] Although the Fe element was removed in Comparative Example 3, due to the lack of hydroxide addition during the chelation process between EDTA and iron ions, the material showed uneven grain growth during the sintering process, and the specific capacity and cycle performance decreased;
[0118] Compared with Comparative Example 5, the specific capacity and capacity retention rate of the materials in Examples 1-3 are similar, but Comparative Example 5 uses high-purity raw materials, and the unit price of 99.8% sodium carbonate is 80-90 yuan / kg, and the unit price of 99.9% diammonium phosphate is 50-90 yuan / kg. The unit price of industrial-grade sodium carbonate is 1.5-3 yuan / kg, and the price of industrial-grade diammonium phosphate is 1-5 yuan / kg. It can be seen that when the preparation process provided by the present invention is adopted, the cost is reduced by 70-90% on the basis of ensuring the performance of the material; at the same time, in Examples 1-3, reagents one and two are used for impurity removal, which may be due to the synergistic effect of hydroxide ions and divalent alkali metal cations, so as to improve the uniformity and stability of material sintering, and improve the specific capacity and cycle stability of the material.
[0119] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a titanium-based phosphate active material, characterized in that: The following steps are involved: S1, dissolving a precursor raw material in a solvent and dispersing it with a dispersant to obtain a mixed solution; the precursor raw material includes a soluble sodium source, a soluble phosphorus source and an organic carbon source; S2, reacting the mixed solution of step S1 with reagent 1 and reagent 2, and separating the precipitate and the solution after the reaction is completed; S3, grinding the titanium source with D50=10-20 μm to make it D50=1-5 μm, mixing the ground titanium source with the solution separated in step S2 and the inorganic carbon source to obtain a mixed slurry, and wet grinding the mixed slurry to reduce the particle size of D50<1 μm to obtain a precursor slurry; S4, spray drying the precursor slurry in step S3 to obtain a precursor powder; S5, sintering the precursor powder of step S4 under an inert atmosphere; S6, crushing the product sintered in step S5, demagnetizing it, and obtaining the titanium-based phosphate active material; The sodium source and phosphorus source are industrial pure raw materials, and the purity of the titanium source is >99%; The reagent 1 is selected from sodium hydroxide or ammonia water, and the reagent 2 is selected from one or more of barium carbonate, barium chloride, calcium chloride and calcium hydroxide.
2. The preparation method according to claim 1, characterized in that: The molar ratio of the reagent 1 to the sodium source is (0.02-0.1):1, and the molar ratio of the reagent 2 to the sodium source is (0.02-0.1):1; The molar ratio of the sodium source, the phosphorus source and the titanium source is 1:3-5:1-2.
3. The preparation method according to claim 1, characterized in that: Preferably, the soluble sodium source is selected from one or more of sodium carbonate, sodium phosphate, sodium oxalate, sodium acetate, sodium formate, and sodium citrate; Preferably, the soluble phosphorus source is selected from one or more of monoammonium phosphate, diammonium phosphate, orthophosphoric acid, metaphosphoric acid, phosphoric acid, and sodium pyrophosphate; Preferably, the titanium source comprises titanium dioxide.
4. The preparation method according to claim 1, characterized in that: Preferably, the organic carbon source is selected from one or more of glucose, sucrose, polyvinyl alcohol compounds, citric acid, and polyacrylic acid compounds; Preferably, the molar ratio of the organic carbon source to the sodium source is (0.01-0.5):1; Preferably, the inorganic carbon source is selected from one or more of conductive carbon black, acetylene black, Ketjen black, artificial graphite, natural graphite, carbon fiber, carbon nanotube dry powder, graphene, and carbon nanotube aqueous dispersion; Preferably, the molar ratio of the inorganic carbon source to the sodium source is (0.01-0.5):
1.
5. The preparation method according to claim 1, characterized in that: In step S1: Preferably, the dispersant is an inorganic alkali metal phosphate compound and / or an organic polymer compound; Preferably, the amount of the dispersant used is 0.1-2 wt % of the precursor raw material.
6. The preparation method according to claim 1, characterized in that: In step S3, preferably, the pulverization is air flow pulverization.
7. The preparation method according to claim 1, characterized in that: In step S4, the spray drying is performed at an air inlet temperature of 180-240°C, an air outlet temperature of 90-120°C, and a centrifugal speed of 25000-35000 r / min.
8. The preparation method according to claim 1, characterized in that: In step S5, the sintering is to heat the precursor powder to 300-400°C at a heating rate of 1-10°C / min and keep it at that temperature for 1-5 hours, and then further heat it to 600-800°C at a heating rate of 1-10°C / min and calcine it for 5-10 hours.
9. The electrode active material obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The structural formula of the electrode active material is Na a Ti b X c , wherein X is a phosphate group, a=1-2, b=1-2, c=3-5.
10. An electrode plate, characterized in that: The invention comprises an electrode active layer, wherein the electrode active layer comprises the electrode active material according to claim 9, a conductive agent and a binder.
Citation Information
Patent Citations
Carbon coated prepared titanium phosphate sodium material and preparation and application
CN108615855A
Preparation method of sodium titanium phosphate material
CN109205585A
Preparation method of water-based processing ferric sodium pyrophosphate
CN116986569A
Iron-based polyphosphate type sodium ion battery positive electrode material as well as preparation method and application thereof
CN117794854A
Composite material for water-based sodium-ion battery and preparation method of composite material
CN117878294A