Silicon-carbon negative electrode material and preparation method and application thereof

Through self-assembly and high-temperature pyrolysis of modified microcrystalline graphite and silicon waste, silicon-carbon anode materials with high conductivity and cycle stability are prepared, which solves the problems of high cost and short life of silicon-carbon composite materials in lithium-ion batteries. problem, improving the overall performance of the battery.

CN118754115AActive Publication Date: 2024-10-11KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410924643.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-11
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Silicon-carbon composite materials have problems such as high production cost, poor cycle life, low conductivity and large volume expansion in batteries, which affects their application in lithium-ion batteries.

Method used

By modifying and self-assembling copper salts, microcrystalline graphite and silicon waste, copper-doped silicon-carbon microspheres are formed, and silicon-carbon negative electrode materials are obtained through high-temperature pyrolysis to improve its conductivity and cycle stability.

Benefits of technology

It reduces the production cost of battery materials, significantly improves the conductivity and cycle stability of silicon-carbon anode materials, slows down the volume expansion during charge and discharge, and improves the cycle performance and first Coulomb efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754115A_ABST
    Figure CN118754115A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery negative electrodes, in particular to a silicon-carbon negative electrode material and a preparation method and application thereof. The preparation method comprises the following steps: firstly modifying microcrystalline graphite to obtain modified graphite, then combining the modified microcrystalline graphite, a silicon waste suspension and a carbon source, carrying out self-assembly, and then carrying out pyrolysis to prepare the silicon-carbon negative electrode material. The material has high tap density, high first coulombic efficiency and high cycle performance, can greatly slow down autogenous volume expansion of the silicon material in the charging and discharging process, and improves the cycle stability of the battery. The method is low in raw material requirement and simple in equipment requirement; the used waste silicon material and microcrystalline graphite are low in price, the silicon-carbon negative electrode material can be continuously and industrially produced at low cost, and a potential scheme is provided for large-scale production of the silicon-based negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery negative electrodes, and in particular to a silicon-carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] Silicon has an extremely high theoretical specific capacity and is often regarded as a potential high-specific capacity negative electrode material. However, during the use of silicon, the battery capacity decays rapidly, and there are also problems such as large volume expansion, low conductivity, and slow ion diffusion.

[0003] At present, the performance of silicon negative electrode materials is often improved by nano-sizing, and the combination of silicon with metals and active or inactive materials. Among them, silicon-carbon composite materials are the main technical route. However, the preparation of silicon-carbon materials is complex, the cycle life is poor, and the cost is high. Summary of the invention

[0004] The purpose of the present invention is to provide a silicon-carbon negative electrode material and a preparation method and application thereof, so as to reduce production costs and improve the conductivity and cycle stability of the silicon negative electrode material.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] A method for preparing a silicon-carbon negative electrode material comprises the following steps

[0007] 1) mixing copper salt, water, microcrystalline graphite dispersion and precipitant, and modifying to obtain modified microcrystalline graphite;

[0008] 2) mixing the modified microcrystalline graphite, silicon waste and carbon source, and performing self-assembly to obtain copper-doped silicon-carbon microspheres;

[0009] 3) Pyrolyzing the copper-doped silicon-carbon microspheres to obtain the silicon-carbon negative electrode material.

[0010] Optionally, the copper salt in step 1) comprises at least one of Cu(NO3)2·3H2O, CuSO4·5H2O or CuCl2.

[0011] Optionally, the precipitant in step 1) comprises at least one of NH4HCO3, NaOH, NaCO3 or HCl; the mass ratio of microcrystalline graphite to precipitant in the copper salt, water and microcrystalline graphite dispersion is 1-3:8-20:2-4:1-3.

[0012] Optionally, the modification temperature in step 1) is 50-100° C. and the time is 30-120 min.

[0013] Optionally, in step 2), the concentration of silicon waste in the silicon waste suspension is 0.02-0.3 g / mL; the carbon source comprises at least one of nanocellulose, carbon nanotubes, sucrose, glucose, dopamine or asphalt; and the mass ratio of silicon waste to carbon source in the modified microcrystalline graphite, silicon waste and silicon waste suspension is 1-5:1-6:0.2-1.5.

[0014] Optionally, the temperature of the self-assembly in step 2) is 100-200°C.

[0015] Optionally, the pyrolysis temperature in step 3) is 700-3000° C. and the pyrolysis time is 0.1-12 h.

[0016] The invention provides a silicon-carbon negative electrode material prepared by the preparation method.

[0017] The present invention also provides application of the silicon-carbon negative electrode material in a lithium ion battery.

[0018] The present invention provides a method for preparing a silicon-carbon negative electrode material. Specifically, according to the structural characteristics of microcrystalline graphite and silicon waste, the microcrystalline graphite and waste silicon material are first physically crushed to improve the particle size. The reduced particle size can effectively alleviate the volume expansion of silicon and enhance the composite of silicon and microcrystalline graphite; then a layer of copper is deposited on the surface of the microcrystalline graphite by chemical deposition to modify the surface of the microcrystalline graphite. The acid-base neutralization reaction of copper can deposit a layer of copper compound on the surface of the microcrystalline graphite, which can improve the surface defects of the microcrystalline graphite itself. At the same time, the excellent conductivity and high relative atomic mass of copper can improve the conductivity and tap density of the silicon composite material; finally, the modified microcrystalline graphite and waste silicon powder are subjected to controllable spray granulation carbon coating treatment and high-temperature pyrolysis to obtain the silicon-carbon negative electrode material of the present invention.

[0019] In the silicon-carbon negative electrode material described in the present invention, silicon particles are attached to the surface of modified microcrystalline graphite and are surface-coated by a carbon source. Silicon and graphite are effectively compounded, which can not only reduce unnecessary electrolyte decomposition on the electrode surface, but also help maintain good electrode integrity during the cycle process, so that the material has a high first coulombic efficiency and high cycle performance, and can greatly slow down the spontaneous volume expansion of the silicon material during the charge and discharge process, thereby improving the cycle stability of the battery.

[0020] The improvement of particle size and carbon coating strategy in the present invention can effectively inhibit the volume expansion of silicon, reduce the side reaction between silicon and electrolyte, and improve the initial coulombic efficiency and cycle stability of the composite material. The quality improvement brought by copper doping and the refinement of material particle size jointly improve the tap density of the composite material.

[0021] The present invention has low requirements for raw materials, simple equipment requirements, easy operation and easy to scale up; the waste silicon materials and microcrystalline graphite used are inexpensive and can be produced continuously in an industrialized manner at low cost; it can effectively recycle crystalline silicon waste in the photovoltaic industry, and can also effectively prepare high-initial-efficiency and high-tap-density spherical silicon-carbon negative electrode materials, providing a potential solution for the large-scale production of silicon-based negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of the method for preparing the silicon-carbon negative electrode material;

[0023] Figure 2 This is a morphology diagram of the silicon-carbon negative electrode material prepared in Example 1;

[0024] Figure 3 This is a morphology diagram of the silicon-carbon negative electrode material prepared in Example 2;

[0025] Figure 4 This is a morphology diagram of the silicon-carbon negative electrode material prepared in Example 3;

[0026] Figure 5 This is a morphology diagram of the silicon-carbon negative electrode material prepared in Example 4;

[0027] Figure 6 This is a cycling performance diagram of the morphology diagram of the silicon-carbon negative electrode material prepared in Example 5. DETAILED DESCRIPTION

[0028] like Figure 1 As shown, the present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps:

[0029] 1) mixing copper salt, water, microcrystalline graphite dispersion and precipitant, and modifying to obtain modified microcrystalline graphite;

[0030] 2) mixing the modified microcrystalline graphite, silicon waste suspension and carbon source, and performing self-assembly to obtain copper-doped silicon-carbon microspheres;

[0031] 3) Pyrolyzing the copper-doped silicon-carbon microspheres to obtain the silicon-carbon negative electrode material.

[0032] In the present invention, the microcrystalline graphite in step 1) is preferably refined by grinding; the particle size of the refined microcrystalline graphite is preferably 0.05 to 5 μm, and more preferably 0.1 to 4.5 μm;

[0033] The grinding preferably uses a crusher and a sand mill in sequence. The use conditions of the crusher are not particularly limited, and any crushing can be completed; the speed of the sand mill is preferably 2000-2800 r / min, more preferably 2100-2500 r / min, and more preferably 2200-2400 r / min; the sand milling time is preferably 2-12 h, more preferably 3-10 h, more preferably 4-8 h, and more preferably 5-6 h; the sand milling medium is preferably water, an aqueous solution or an alcohol solution, and more preferably anhydrous ethanol;

[0034] The refined microcrystalline graphite is dried and dispersed in water to obtain a microcrystalline graphite dispersion;

[0035] The drying conditions are not particularly limited, and any conditions that can achieve drying are acceptable. The concentration of the microcrystalline graphite dispersion is preferably 0.25 to 0.5 g / mL.

[0036] In the present invention, the copper salt in step 1) preferably comprises at least one of Cu(NO3)2·3H2O, CuSO4·5H2O or CuCl2.

[0037] In the present invention, the precipitant in step 1) preferably comprises at least one of NH4HCO3, NaOH, NaCO3 or HCl; the mass ratio of microcrystalline graphite and precipitant in the copper salt, water and microcrystalline graphite dispersion is preferably 1-3:8-20:2-4:1-3, further preferably 1-2:8-15:2-3:1-2, and further preferably 1-2:10-12:2-3:1-2.

[0038] In the present invention, the temperature of the modification in step 1) is preferably 50-100°C, more preferably 60-90°C, and even more preferably 70-80°C; the time is preferably 30-120 min, and even more preferably 60-90 min.

[0039] In the present invention, the mixing in step 1) is preferably to mix the copper salt with water, then add the microcrystalline graphite dispersion, heat, and when the temperature rises to 100° C., dropwise add the precipitant solution;

[0040] Step 1) The modification is preferably performed by stirring at a constant temperature after the precipitant solution is added dropwise, allowing the reaction to proceed fully. After the reaction is completed, the mixture is filtered and washed several times with deionized water to obtain modified microcrystalline graphite.

[0041] In the present invention, the silicon waste in step 2) preferably includes silicon cutting waste of solar cell sheets in the photovoltaic industry;

[0042] The silicon waste suspension is preferably refined by sand milling, and the refined medium is a silicon waste suspension in anhydrous ethanol; the particle size of the refined silicon waste is preferably 0.05 to 5 μm, more preferably 0.1 to 4.5 μm; the particle size of the refined microcrystalline graphite is preferably 0.05 to 5 μm, more preferably 0.1 to 4.5 μm;

[0043] The grinding preferably uses a crusher and a sand mill in sequence. The use conditions of the crusher are not particularly limited, and any method that can complete the crushing is acceptable; the speed of the sand mill is preferably 2000-2800 r / min, more preferably 2100-2500 r / min, and further preferably 2200-2400 r / min; the sand milling time is preferably 2-12 h, more preferably 3-10 h, more preferably 4-8 h, and further preferably 5-6 h; the sand milling medium is preferably water, an aqueous solution or an alcohol solution, and further preferably anhydrous ethanol.

[0044] In the present invention, the concentration of silicon waste in the silicon waste suspension in step 2) is preferably 0.02-0.3 g / mL, more preferably 0.025-0.1 g / mL, and further preferably 0.035-0.04 g / mL; the carbon source preferably comprises at least one of nanocellulose, carbon nanotubes, sucrose, glucose, dopamine or asphalt. When the carbon source is two or more of the above, the ratio between the carbon sources can be adjusted according to actual conditions; the mass ratio of silicon waste and carbon source in the modified microcrystalline graphite and silicon waste suspension is preferably 1-5:1-6:0.2-1.5, further preferably 1-4:1.2-4:0.25-1, and further preferably 2-3:2-3:0.3-0.6.

[0045] In the present invention, the temperature of the self-assembly in step 2) is preferably 100-200°C, more preferably 110-150°C, and even more preferably 120-130°C.

[0046] In the present invention, the feeding rate of the precursor solution in the self-assembly process of step 2) is preferably 0.1-33 mL / min, more preferably 5-15 mL / min, and further preferably 8-10 mL / min; the assembly process preferably requires the introduction of gas, and the gas is preferably at least one of nitrogen, argon or air; the gas feeding rate is preferably 0.1-100 mL / min, more preferably 5-15 mL / min, and further preferably 8-10 mL / min.

[0047] In the present invention, the pyrolysis temperature in step 3) is preferably 700-3000°C, more preferably 800-1500°C, and further preferably 1000-1300°C; the pyrolysis time is preferably 0.1-12h, more preferably 2-8h, and further preferably 4-6h.

[0048] In the present invention, in step 3), argon is preferably introduced into the pyrolysis, and its flow rate is preferably 5-20 mL / min, and more preferably 10-15 mL / min; the heating rate of the pyrolysis is preferably 0.1-20°C / min, more preferably 3-15°C / min, and even more preferably 5-10°C / min.

[0049] The invention provides a silicon-carbon negative electrode material prepared by the preparation method.

[0050] The present invention also provides the application of the silicon-carbon negative electrode material in a lithium-ion battery; the present invention has no special limitation on the method of the application, and any application method can be used in a lithium-ion battery.

[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0052] Example 1

[0053] (1) using a crusher to refine the waste silicon material and microcrystalline graphite raw materials, and then further grinding them to submicron level with a sand mill, using anhydrous ethanol as the sand mill grinding medium, the sand mill speed is controlled at 2800r / min, the sand milling time is controlled at 3h, and the particle size distribution of the refined waste silicon material and microcrystalline graphite is 0.05-5μm; after the waste silicon material is sand milled, a silicon waste suspension is obtained, and its concentration is 0.04g / mL;

[0054] (2) drying the sand-ground microcrystalline graphite in a vacuum drying oven at 60° C., taking 100 g of the microcrystalline graphite and dispersing it in 200 mL of deionized water to obtain a 0.5 g / mL microcrystalline graphite dispersion;

[0055] 25 g of Cu(NO3)2·3H2O and 200 mL of deionized water were mixed and placed in a beaker, and magnetic stirring was performed for 15 min. 100 mL of the microcrystalline graphite dispersion (0.5 g / mL) was added, and the mixture was stirred evenly and heated. When the temperature rose to 100°C, 500 mL of NH4HCO3 solution (mass concentration was 0.05 g / mL) was added dropwise. After the addition was completed, constant temperature stirring was performed for 60 min to fully react. After the reaction was completed, the mixture was filtered and washed with deionized water to obtain modified microcrystalline graphite;

[0056] (3) 19.2 g of the modified microcrystalline graphite obtained in step (2), 600 mL of the refined silicon waste suspension (0.04 g / mL) obtained in step (1), 2.4 g of asphalt and 2.4 g of nanocellulose were mixed to obtain a precursor solution;

[0057] The precursor solution was added at a feed rate of 10 mL / min, nitrogen was introduced at a gas feed rate of 10 mL / min, and spray granulation self-assembly was performed in a spray granulator at 150° C. for 1 h to obtain copper-doped silicon-carbon microspheres;

[0058] (4) The copper-doped silicon-carbon microspheres obtained in step (3) were placed in a tubular furnace, argon gas was introduced at a flow rate of 10 mL / min, and then heated to 700°C at a heating rate of 5°C / min for pyrolysis for 2 h to obtain a silicon-carbon negative electrode material.

[0059] Example 2

[0060] (1) using a crusher to refine the waste silicon material and microcrystalline graphite raw materials, and then further grinding them to submicron level with a sand mill, using anhydrous ethanol as the sand mill grinding medium, the sand mill speed is controlled at 2400r / min, the sand milling time is controlled at 8h, and the particle size distribution of the refined waste silicon material and microcrystalline graphite is 0.05-5μm; after the waste silicon material is sand milled, a silicon waste suspension is obtained, and its concentration is 0.1g / mL;

[0061] (2) drying the sand-ground microcrystalline graphite in a vacuum drying oven at 60° C., taking 100 g of the microcrystalline graphite and dispersing it in 200 mL of deionized water to obtain a 0.5 g / mL microcrystalline graphite dispersion;

[0062] 12 g of Cu(NO3)2·3H2O and 96 mL of deionized water were mixed and placed in a beaker, and magnetic stirring was performed for 15 min. 48 mL of the microcrystalline graphite dispersion (0.5 g / mL) was added, and the mixture was stirred evenly and heated. When the temperature rose to 100°C, 100 mL of NH4HCO3 solution (with a concentration of 0.12 g / mL) was added dropwise. After the addition was completed, the mixture was stirred at a constant temperature for 60 min to fully react. After the reaction was completed, the mixture was filtered and washed with deionized water to obtain modified microcrystalline graphite;

[0063] (3) 12 g of the modified microcrystalline graphite obtained in step (2), 240 mL of the refined silicon waste suspension (0.1 g / mL) obtained in step (1), 0.8 g of asphalt and 3.2 g of nanocellulose were mixed to obtain a precursor solution;

[0064] The precursor solution was added at a feed rate of 8 mL / min, nitrogen was introduced at a gas feed rate of 5 mL / min, and spray granulation self-assembly was performed in a spray granulator at 120° C. for 30 min to obtain copper-doped silicon-carbon microspheres;

[0065] (4) The copper-doped silicon-carbon microspheres obtained in step (3) were placed in a tubular furnace, argon gas was introduced at a flow rate of 15 mL / min, and then heated to 1300°C at a heating rate of 10°C / min for pyrolysis for 4 h to obtain a silicon-carbon negative electrode material.

[0066] Example 3

[0067] (1) using a crusher to refine the waste silicon material and microcrystalline graphite raw materials, and then further grinding them to submicron level with a sand mill, using anhydrous ethanol as the sand mill grinding medium, the sand mill speed is controlled at 2000r / min, the sand milling time is controlled at 10h, and the particle size distribution of the refined waste silicon material and microcrystalline graphite is 0.05-5μm; after the waste silicon material is sand milled, a silicon waste suspension is obtained, and its concentration is 0.025g / mL;

[0068] (2) drying the sand-milled microcrystalline graphite in a vacuum drying oven at 60° C., taking 100 g of the microcrystalline graphite and dispersing it in 400 mL of deionized water to obtain a 0.25 g / mL microcrystalline graphite dispersion;

[0069] 24 g of CuSO4·5H2O and 192 mL of deionized water were mixed and placed in a beaker, and magnetically stirred for 15 min. 192 mL of the microcrystalline graphite dispersion (0.25 g / mL) was added, and the mixture was stirred evenly and heated. When the temperature rose to 100° C., 60 mL of NaOH solution (mass concentration was 40%) was added dropwise. After the addition was completed, the mixture was stirred at a constant temperature for 60 min to fully react. After the reaction was completed, the mixture was filtered and washed with deionized water to obtain modified microcrystalline graphite;

[0070] (3) mixing 16 g of the modified microcrystalline graphite obtained in step (2), 800 mL of the refined silicon waste suspension (0.025 g / mL) obtained in step (1), and 4 g of asphalt to obtain a precursor solution;

[0071] The precursor solution was added at a feed rate of 15 mL / min, nitrogen was introduced at a gas feed rate of 10 mL / min, and spray granulation self-assembly was performed in a spray granulator at 130° C. for 80 min to obtain copper-doped silicon-carbon microspheres;

[0072] (4) The copper-doped silicon-carbon microspheres obtained in step (3) were placed in a tubular furnace, argon gas was introduced at a flow rate of 5 mL / min, and then heated to 1300°C at a heating rate of 10°C / min for pyrolysis for 4 h to obtain a silicon-carbon negative electrode material.

[0073] Example 4

[0074] (1) using a crusher to refine the waste silicon material and microcrystalline graphite raw materials, and then further grinding them to submicron level with a sand mill, using anhydrous ethanol as the sand mill grinding medium, the sand mill speed is controlled at 2500r / min, the sand milling time is controlled at 6h, and the particle size distribution of the refined waste silicon material and microcrystalline graphite is 0.05-5μm; after the waste silicon material is sand milled, a silicon waste suspension is obtained, and its concentration is 0.035g / mL;

[0075] (2) drying the sand-milled microcrystalline graphite in a vacuum drying oven at 60° C., taking 150 g of the microcrystalline graphite and dispersing it in 300 mL of deionized water to obtain a 0.5 g / mL microcrystalline graphite dispersion;

[0076] 12 g of CuSO4·5H2O and 96 mL of deionized water were mixed and placed in a beaker, and magnetically stirred for 15 min. 48 mL of the microcrystalline graphite dispersion (0.5 g / mL) was added, and the mixture was stirred evenly and heated. When the temperature rose to 100° C., 60 mL of NaOH solution (with a concentration of 20%) was added dropwise. After the addition was completed, the mixture was stirred at a constant temperature for 60 min to fully react. After the reaction was completed, the mixture was filtered and washed with deionized water to obtain modified microcrystalline graphite;

[0077] (3) mixing 21 g of the modified microcrystalline graphite obtained in step (2), 1000 mL of the refined silicon waste suspension (0.035 g / mL) obtained in step (1), 3.5 g of asphalt and 3.5 g of nanocellulose to obtain a precursor solution;

[0078] The precursor solution was added at a feed rate of 8 mL / min, nitrogen was introduced at a gas feed rate of 8 mL / min, and spray granulation self-assembly was performed in a spray granulator at 110° C. for 100 min to obtain copper-doped silicon-carbon microspheres;

[0079] (4) The copper-doped silicon-carbon microspheres obtained in step (3) were placed in a tubular furnace, argon gas was introduced at a flow rate of 15 mL / min, and then heated to 1000°C at a heating rate of 5°C / min for pyrolysis for 8 h to obtain a silicon-carbon negative electrode material.

[0080] Example 5

[0081] (1) using a crusher to refine the waste silicon material and microcrystalline graphite raw materials, and then further grinding them to submicron level with a sand mill, using anhydrous ethanol as the grinding medium, the sand mill speed is controlled at 2500r / min, the sand mill time is controlled at 4h, and the particle size distribution of the refined waste silicon material and microcrystalline graphite is 0.05-5μm; after the waste silicon material is sand milled, a silicon waste suspension is obtained, and its concentration is 0.05g / mL;

[0082] (2) drying the sand-ground microcrystalline graphite in a vacuum drying oven at 60° C., taking 100 g of the microcrystalline graphite and dispersing it in 200 mL of deionized water to obtain a 0.5 g / mL microcrystalline graphite dispersion;

[0083] 12 g of Cu(NO3)2·3H2O and 200 mL of deionized water were mixed and placed in a beaker, and magnetic stirring was performed for 15 min. 100 mL of the microcrystalline graphite dispersion (0.5 g / mL) was added, and the mixture was stirred evenly and heated. When the temperature rose to 100°C, 100 mL of NH4HCO3 solution (with a concentration of 4.8 g / L) was added dropwise. After the addition was completed, the mixture was stirred at a constant temperature for 60 min to fully react. After the reaction was completed, the mixture was filtered and washed with deionized water to obtain modified microcrystalline graphite;

[0084] (3) 20 g of the modified microcrystalline graphite obtained in step (2), 500 mL of the refined silicon waste suspension (0.05 g / mL) obtained in step (1), 1 g of asphalt and 4 g of nanocellulose were mixed in a mass ratio of 4:5:0.2:0.8 to obtain a precursor solution;

[0085] The precursor solution was added at a feed rate of 10 mL / min, nitrogen was introduced at a gas feed rate of 15 mL / min, and spray granulation self-assembly was performed in a spray granulator at 130° C. for 50 min to obtain copper-doped silicon-carbon microspheres;

[0086] (4) The copper-doped silicon-carbon microspheres obtained in step (3) were placed in a tubular furnace, argon gas was introduced at a flow rate of 15 mL / min, and then heated to 800°C at a heating rate of 3°C / min for pyrolysis for 6 h to obtain a silicon-carbon negative electrode material.

[0087] Test Case

[0088] The morphology of the silicon-carbon negative electrode materials prepared in Examples 1 to 4 was detected using a field emission scanning electron microscope. The results are as follows: Figures 1 to 4 As shown;

[0089] in, Figure 2 This is a morphology diagram of the silicon-carbon negative electrode material obtained in Example 1;

[0090] pass Figure 2 It can be found that the overall morphology of the silicon-carbon negative electrode material prepared in Example 1 is spherical, with a smooth surface and some pellets have defects;

[0091] Figure 3 This is a morphology diagram of the silicon-carbon negative electrode material obtained in Example 2;

[0092] pass Figure 3 It can be found that the silicon-carbon negative electrode material prepared in Example 2 has high sphericity, uniform morphology, and a smooth and dense surface;

[0093] Figure 4 This is a morphology diagram of the silicon-carbon negative electrode material obtained in Example 3;

[0094] pass Figure 4 It can be found that the silicon-carbon negative electrode material prepared in Example 3 has high sphericity and a smooth surface;

[0095] Figure 5 This is a morphology diagram of the silicon-carbon negative electrode material obtained in Example 4;

[0096] pass Figure 5 It can be found that the silicon-carbon negative electrode material prepared in Example 4 is basically spherical, and defects can be seen on the surface of a few pellets.

[0097] The tap density of the silicon-carbon negative electrode materials prepared in Examples 1 to 5 was tested using a Yuntang YZ-ZS1 tap density meter; the silicon-carbon negative electrode materials prepared in Examples 1 to 5 were used for button battery testing, lithium sheets were used as the electrode material, the electrolyte was 1.5MLiTFSI in EC:DEC=1:1Vo1%with 5.0%FEC, and the test system was a Xinwei battery test system. The first coulomb efficiency, the first discharge specific capacity, and the charge and discharge cycle effect after 150 times were tested at 0.2A / g. The results are shown in Table 1:

[0098] Table 1 Performance test of silicon-carbon negative electrode materials prepared in Examples 1 to 5

[0099]

[0100] The silicon-carbon negative electrode material prepared in Example 5 was subjected to a cycle performance test, and the results are as follows: Figure 6 As shown;

[0101] pass Figure 6 It can be found that the silicon-carbon negative electrode material has excellent cycle performance. When tested under a current density of 0.2 A / g, the initial discharge capacity is 2624 mAh / g, and the remaining capacity is 1592 mAh / g after 150 charge and discharge cycles.

[0102] Through Table 1 and Figure 6 It can be found that the tap density of the silicon-carbon negative electrode material prepared by the present invention can reach 0.91 g / cm 3 The first coulombic efficiency can reach 89.8%, the first discharge specific capacity is 2901mAh / g, and the remaining capacity can reach 1825mAh / g after 150 charge and discharge cycles, with good real density and cycle stability.

[0103] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: The following steps are included 1) mixing copper salt, water, microcrystalline graphite dispersion and precipitant, and modifying to obtain modified microcrystalline graphite; 2) mixing the modified microcrystalline graphite, silicon waste suspension and carbon source, and performing self-assembly to obtain copper-doped silicon-carbon microspheres; 3) Pyrolyzing the copper-doped silicon-carbon microspheres to obtain the silicon-carbon negative electrode material.

2. The preparation method according to claim 1, characterized in that: Step 1) The copper salt comprises at least one of Cu(NO3)2·3H2O, CuSO4·5H2O or CuCl2.

3. The preparation method according to claim 1 or 3, characterized in that: Step 1) The precipitant comprises at least one of NH4HCO3, NaOH, NaCO3 or HCl; the mass ratio of the microcrystalline graphite to the precipitant in the copper salt, water and microcrystalline graphite dispersion is 1-3:8-20:2-4:1-3.

4. The preparation method according to claim 4, characterized in that: Step 1) The modification temperature is 50-100°C and the time is 30-120 minutes.

5. The preparation method according to claim 1, characterized in that: Step 2) The concentration of silicon waste in the silicon waste suspension is 0.02-0.3 g / mL; the carbon source comprises at least one of nanocellulose, carbon nanotubes, sucrose, glucose, dopamine or asphalt; the mass ratio of the modified microcrystalline graphite, silicon waste and carbon source in the silicon waste suspension is 1-5:1-6:0.2-1.

5.

6. The preparation method according to claim 1, characterized in that: Step 2) The temperature of the self-assembly is 100-200°C.

7. The preparation method according to claim 1, characterized in that: Step 3) The pyrolysis temperature is 700-3000°C; the pyrolysis time is 0.1-12h.

8. The silicon-carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the silicon-carbon negative electrode material according to claim 8 in lithium-ion batteries.

Citation Information

Patent Citations

  • Preparation method of silicon / carbon / graphite composite material for lithium ion battery cathode

    CN110048097A

  • Preparation method and application of low-cost silicon graphite negative electrode active material

    CN117096329A