Sodium-ion battery Prussian blue positive electrode material and preparation method thereof

By adding organic sulfur-containing compounds and performing a hydrothermal reaction during the synthesis process of Prussian blue cathode material, combined with the coating of graphene oxide, the problems of lattice defects and poor conductivity of the material were solved, and a high-quality Prussian blue cathode was achieved Material preparation.

CN118754153APending Publication Date: 2024-10-11SHENZHEN TECH UNIV

Patent Information

Application Number
CN202410126867.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Prussian blue cathode materials are prone to lattice defects and large crystal moisture during the synthesis process, resulting in poor conductivity and affecting the performance of sodium-ion batteries.

Method used

By adding an organic sulfur-containing compound complexing agent and performing a hydrothermal reaction during the synthesis process to reduce the crystallization rate, and using reduced graphene oxide for coating, the lattice defects and moisture content of the material are reduced.

Benefits of technology

It significantly improves the conductivity and stability of the Prussian blue cathode material, and solves the problems of structural distortion and insufficient conductivity of the material during the charge and discharge process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754153A_ABST
    Figure CN118754153A_ABST
Patent Text Reader

Abstract

The invention relates to the field of battery positive electrode materials, and discloses a preparation method of a sodium ion battery Prussian blue positive electrode material, which comprises the following steps: (1) respectively dissolving transition metal salt TMGI2 and Na4M (CN) 6 in deionized water, adding an organic sulfur-containing compound into the transition metal salt TMCI2 solution, after the organic sulfur-containing compound is fully dissolved, dropwise adding the transition metal salt solution into the Na4M (CN) 6, and stirring to obtain a mixed solution; after titration is completed, centrifuging to obtain PBAs; and (2) dispersing the PBAs prepared in the step (1) into deionized water, adding graphene oxide, then putting the mixture into a reaction kettle for hydrothermal reaction, and obtaining a sample rGO-coated PBAs loaded with reduced graphene oxide after the reaction is finished. The preparation of the high-quality Prussian blue positive electrode material is realized, and the method is simple in process and remarkable in effect, and is a method for reducing lattice defects, material conductivity and stability of the Prussian blue positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cathode materials for batteries, and particularly to a sodium-ion battery Prussian blue cathode material and a preparation method thereof. Background Art

[0002] In recent years, with the increasing scarcity of lithium resources and the continuous rise of lithium prices, sodium-ion batteries have attracted wide attention due to advantages such as abundant sodium reserves, wide distribution, and low cost. The relatively wide operating temperature range and high safety make sodium-ion batteries stand out in the energy storage field. Prussian blue analogues (PBAs) have become one of the most ideal cathode materials for sodium-ion batteries due to their open framework structure, abundant redox active centers, and excellent structural stability. Generally, PBAs are represented by A x TM y [M(CN)6] z Z m ·nH2O (when there are anionic [Fe(CN)6] / [Mn(CN)6] vacancies, 0 < x ≤ 2; 0 < y ≤ 1, z + m = 1; when there are cationic TM vacancies, 0 < z ≤ 1, y + m = 1), where A, TM, and Z are mobile alkali metal ions, transition metal ions, and vacancies respectively, and M is Fe or Mn.

[0003] The synthesis of PBAs usually adopts the traditional chemical precipitation method. In this process, the inevitable generation of defect vacancies during rapid crystal nucleation brings a series of problems, such as destroying the integrity of the M-CN-TM bridging structure, causing structural distortion and collapse of the material during charge and discharge, and hindering the conduction of electrons along the material framework, weakening the conductivity of the material. In addition, after the vacancies are occupied by interstitial water, the diffusion of alkali metal ions is blocked, weakening the rate performance of the battery during charge and discharge. Summary of the Invention

[0004] The purpose of the present invention is to provide a sodium-ion battery Prussian blue cathode material and a preparation method thereof, which reduce the synthesis rate of PBAs by adding an organic sulfur-containing compound complexing agent, reduce the lattice defects and moisture content of the material, and coat it with reduced graphene oxide to solve the problems of large lattice defects, large crystallization moisture, and poor conductivity of the Prussian blue cathode material at the same time.

[0005] In the first aspect, the present application provides a preparation method of a sodium-ion battery Prussian blue cathode material, comprising the following steps:

[0006] (1) Dissolve transition metal salt TMCl2 and Na4M(CN)6 in deionized water respectively, add an organic sulfur-containing compound to the transition metal salt TMCl2 solution, and after complete dissolution, drop the transition metal salt solution into Na4M(CN)6. After titration, centrifuge to obtain PBAs;

[0007] (2) The PBAs prepared in step (1) are dispersed in deionized water, graphene oxide is added, and then placed in a reactor for hydrothermal reaction. After the reaction is completed, a sample rGO@PBAs loaded with reduced graphene oxide is obtained.

[0008] Furthermore, the transition metal salt TMCl2 is one of MnCl2, FeCl2, CoCl2, NiCl2, CuCl2 and ZnCl2, and Na4M(CN)6 is Na4Fe(CN ) 6 or Na4Mn(CN)6.

[0009] Furthermore, the concentration of the transition metal salts TMCl2 and Na4M(CN)6 is 1.0×10 -4 mol / L~3.0×10 -2 mol / L.

[0010] Furthermore, the organic sulfur-containing compound is a mixture of one or more of sodium butyl xanthate, sodium ethyl xanthate, sodium amyl xanthate and sodium isobutyl xanthate.

[0011] Furthermore, the hydrothermal reaction time is 0.5-48h.

[0012] Furthermore, the hydrothermal reaction temperature is 120-200°C.

[0013] Furthermore, the mass ratio of the graphene oxide to PBAs is 0.1% to 10%.

[0014] In a second aspect, the present application provides a Prussian blue positive electrode material for a sodium ion battery, wherein the Prussian blue positive electrode material for a sodium ion battery is prepared by the preparation method described above.

[0015] Compared with the prior art, the present invention adds an organic sulfur-containing compound complexing agent to reduce the crystallization rate during the synthesis of Prussian blue analogs by coprecipitation, and then recrystallizes and reduces the coating of graphene oxide by hydrothermal reaction, thereby realizing the preparation of high-quality Prussian blue positive electrode materials. The scheme has a simple process and significant effect, and is a method for reducing lattice defects, material conductivity and stability of Prussian blue positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a scanning electron microscope image of the Prussian blue positive electrode material for a sodium ion battery prepared in Example 1 of the present invention;

[0017] Figure 2 This is a particle size distribution diagram of the Prussian blue positive electrode material for a sodium ion battery prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0018] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0019] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0021] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0022] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0023] The implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0024] Reference Figure 1-2 In the first aspect, the present application provides a method for preparing a Prussian blue positive electrode material for a sodium ion battery, comprising the following steps:

[0025] (1) Dissolve transition metal salts TMCl2 and Na4M(CN)6 in deionized water respectively, and add an organic sulfur-containing compound to the transition metal salt TMCl2 solution. After the transition metal salt solution is fully dissolved, drop the transition metal salt solution into Na4M(CN)6. After the titration is completed, centrifuge to obtain PBAs.

[0026] (2) The PBAs prepared in step (1) are dispersed in deionized water, graphene oxide is added, and then placed in a reactor for hydrothermal reaction. After the reaction is completed, a sample rGO@PBAs loaded with reduced graphene oxide is obtained.

[0027] Furthermore, the transition metal salt TMCl2 is one of MnCl2, FeCl2, CoCl2, NiCl2, CuCl2 and ZnCl2, and Na4M(CN)6 is Na4Fe(CN)6 or Na4Mn(CN)6.

[0028] Furthermore, the concentration of the transition metal salts TMCl2 and Na4M(CN)6 is 1.0×10 -4 mol / L~3.0×10 -2 mol / L.

[0029] Furthermore, the organic sulfur-containing compound is a mixture of one or more of sodium butyl xanthate, sodium ethyl xanthate, sodium amyl xanthate and sodium isobutyl xanthate.

[0030] Furthermore, the hydrothermal reaction time is 0.5-48h.

[0031] Furthermore, the hydrothermal reaction temperature is 120-200°C.

[0032] Furthermore, the mass ratio of the graphene oxide to PBAs is 0.1% to 10%.

[0033] In a second aspect, the present application provides a Prussian blue positive electrode material for a sodium ion battery, wherein the Prussian blue positive electrode material for a sodium ion battery is prepared by the preparation method described above.

[0034] Example 1

[0035] The following method is used to prepare the Prussian blue positive electrode material for sodium ion batteries, and the method comprises the following steps:

[0036] (1) MnCl2 and Na4Fe(CN)6 were dissolved in deionized water respectively, and sodium butyl xanthate was added to the MnCl2 solution. After the MnCl2 solution was fully dissolved, the MnCl2 solution was added dropwise to the Na4Fe(CN)6. The concentration of the MnCl2 and Na4Fe(CN)6 was 1.0×10 -4 mol / L, after the titration is completed, PBAs are obtained by centrifugation;

[0037] (2) The PBAs prepared in step (1) are dispersed in deionized water, and graphene oxide is added, with the mass ratio of graphene oxide to PBAs being 4%. The mixture is then placed in a reactor for a hydrothermal reaction. The hydrothermal reaction time is 24 h, and the hydrothermal reaction temperature is 170° C. After the reaction is completed, a sample rGO@PBAs loaded with reduced graphene oxide is obtained.

[0038] The present application adds an organic sulfur-containing compound complexing agent to reduce the crystallization rate during the synthesis of Prussian blue analogs using a coprecipitation method, and then recrystallizes and reduces the coating of graphene oxide through a hydrothermal reaction, thereby achieving the preparation of high-quality Prussian blue positive electrode materials. The solution has a simple process and significant effects, and is a method for reducing lattice defects, material conductivity and stability of Prussian blue positive electrode materials.

[0039] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0040] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a Prussian blue positive electrode material for a sodium ion battery, characterized in that: The following steps are included: (1) Dissolve transition metal salts TMCl2 and Na4M(CN)6 in deionized water respectively, and add an organic sulfur-containing compound to the transition metal salt TMCl2 solution. After the transition metal salt solution is fully dissolved, drop the transition metal salt solution into Na4M(CN)6. After the titration is completed, centrifuge to obtain PBAs. (2) The PBAs prepared in step (1) are dispersed in deionized water, graphene oxide is added, and then placed in a reactor for hydrothermal reaction. After the reaction is completed, a sample rGO@PBAs loaded with reduced graphene oxide is obtained.

2. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The transition metal salt TMCl2 is one of MnCl2, FeCl2, CoCl2, NiCl2, CuCl2 and ZnCl2, and Na4M(CN)6 is Na4Fe(CN)6 or Na4Mn(CN)6.

3. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The concentration of the transition metal salts TMCl2 and Na4M(CN)6 is 1.0×10 -4 mol / L~3.0×10 -2 mol / L.

4. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The organic sulfur-containing compound is a mixture of one or more of sodium butyl xanthate, sodium ethyl xanthate, sodium amyl xanthate and sodium isobutyl xanthate.

5. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The hydrothermal reaction time is 0.5-48h.

6. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The hydrothermal reaction temperature is 120-200°C.

7. The method for preparing the Prussian blue positive electrode material for sodium ion battery according to claim 1, characterized in that: The mass ratio of the graphene oxide to PBAs is 0.1% to 10%.

8. A sodium ion battery Prussian blue positive electrode material, characterized in that: The Prussian blue positive electrode material for sodium ion batteries is prepared by the preparation method described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Prussian blue / reduced graphene oxide composite material as well as preparation method and application thereof

    CN104716314A

  • Positive electrode material for sodium-ion battery and preparation method thereof

    CN108046231A

Cited By

  • Ferromanganese precursor, preparation method thereof and positive electrode material