High-entropy Prussian blue positive electrode material of sodium ion battery and preparation method of high-entropy Prussian blue positive electrode material
By introducing the concept of high entropy into the cathode material of sodium-ion batteries and using a uniform mixture of multiple transition metal elements, a high-entropy Prussian blue material was prepared, which solved the limitations of traditional materials in terms of energy density, cycle stability and cost, and significantly Improves the performance and life of sodium-ion batteries while reducing production costs.
Patent Information
- Application Number
- CN202411020792.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional sodium-ion battery cathode materials have limitations in terms of energy density, cycle stability and cost. In particular, Prussian blue materials cannot meet the needs of practical applications in terms of cycle stability and specific capacity.
Using high-entropy Prussian blue cathode material, a variety of transition metal elements (such as ferrous iron, manganese, copper, zinc, tin, cobalt) are added to the raw materials, mixed and precipitated according to a specific stoichiometric ratio, combined with deionized water and A high-entropy Prussian blue material with excellent structural stability was prepared using anhydrous ethanol washing and vacuum drying processes.
It significantly improves the energy density and cycle life of sodium-ion batteries, reduces the production cost of materials, optimizes electrochemical performance and structural stability, and solves the limitations of traditional materials in terms of energy density, cycle stability and cost.
Smart Images

Figure CN118754154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a sodium ion battery high entropy Prussian blue positive electrode material and a preparation method thereof. Background Art
[0002] In recent years, with the increasing problems of energy depletion and environmental degradation, renewable energy such as solar energy, wind energy and tidal energy has been vigorously developed, thus promoting the technical research and development of a series of low-cost new energy storage devices. At present, rechargeable lithium-ion batteries are widely used in portable electronic devices and electric vehicles due to their advantages such as high energy density, high power density and long cycle life. However, the high price, scarce reserves and uneven geographical distribution of lithium resources make it difficult to meet the future market demand growth and further apply them to large-scale energy storage devices. At the same time, four types of electrodes, layered transition metal oxides, polyanionic compounds, organic materials and Prussian blue analogs, have been proven to be used as positive electrode materials for sodium ion batteries. Layered oxides show high reversible specific capacity, but the repulsion between oxygen layers during the cycle causes a large volume expansion of the sodium layer, and the electrolyte solvent will also enter the interlayer structure with sodium ions to co-insert, and its complex phase change mechanism makes this type of material have poor cycle stability; in addition, layered oxides show inherent low working voltage, which reduces the energy density of sodium ion full batteries. Polyanionic compounds exhibit high operating voltage and excellent cycle performance due to their stable structural advantages, but poor electrochemical kinetics and large molecular weight make them have the lowest reversible specific capacity. Organic electrodes with large interlayer spacing break the traditional insertion sodium ion storage mechanism through the strong electron-withdrawing group effect of the edge of the fused aromatic ring, and can contribute high reversible specific capacity due to their multiple active sites; however, the inevitable disadvantage of organic electrodes is that the original materials do not contain sodium ions or are in a sodium-poor state, so the negative electrode materials in the full battery system are required to provide sufficient sodium sources for reversible shuttling between the positive and negative electrodes. In contrast, Prussian blue and its analogs positive electrode materials have long cycle life due to their open three-dimensional framework structure with large interstitial positions and excellent structural stability during charge and discharge; at the same time, their composition and structure are easy to control and change, so they can also achieve high specific capacity and high operating voltage. Therefore, designing a Prussian blue-based positive electrode material that has high specific capacity, high operating voltage, and excellent cycle stability is crucial to optimizing the performance of sodium-ion full batteries, and will also determine the commercialization process of sodium-ion battery technology, which has always been one of the core and frontier areas of energy material research.
[0003] Prussian blue and its analogs are typical metal organic framework materials. The common general molecular formula for sodium ion battery cathode materials is NaxP[R(CN)6]y·nH2O (x≤2, y≤1), where P and R are two transition metal ions connected to N and C, respectively. The material connects two transition metal ions one by one through cyano ligands to form a three-dimensional network framework structure, in which the large interstitial positions can not only store sodium ions, but also provide a three-dimensional transmission channel for their rapid reversible deintercalation; in addition, the two transition metal ions act as redox centers to drive the reversible deintercalation of sodium ions. However, the adsorbed water molecules on the surface of the material, the zeolite and consonant water molecules in the interstitial positions, and the [R(CN)6]4- anion vacancies generated in the structure will deteriorate the sodium ion storage performance. The high content of water molecules not only produces a large irreversible capacity under high voltage, but also causes serious electrode-electrolyte interface reactions; in addition, the [R(CN)6]4- vacancies greatly reduce the content of low-spin active Fe ions that are resonant with C, thereby reducing the specific capacity and causing structural deterioration and lattice collapse during long-term cycles. Studies have shown that the sodium ions in the interstitial position, the resonant water molecules and the content of [R(CN)6]4- vacancies in the structure affect each other. The sodium-rich state will reduce the resonant water content and inhibit the generation of lattice defects; in addition, the content of sodium ions and interstitial water molecules in the molecular formula is closely related to the crystal structure type of the material. As the sodium ion content increases, the structure is cubic, orthorhombic, and monoclinic. The study found that due to the differences in composition and structure, the sodium ion storage mechanism of Prussian blue-based materials mainly includes: solid solution and phase change reaction. This means that the differences in composition factors such as sodium ions, water molecules and [R(CN)6]4- defect content in the interstitial position will further affect whether the electrochemical reaction mechanism is solid solution or phase change process, as well as the specific structural state of the electrode material under different sodium insertion and deintercalation states. Therefore, selecting and adjusting effective material preparation methods and optimizing material composition are of great theoretical significance for achieving controllable regulation of interstitial water molecules and lattice defect content in Prussian blue materials. It will also provide theoretical and experimental basis for constructing the intrinsic connection between defects and structure, performance and reaction mechanism. At the same time, it also has a positive role in optimizing the sodium ion storage performance, explaining the electrochemical reaction mechanism and clarifying its key influencing factors. To this end, we propose a high-entropy Prussian blue positive electrode material for sodium ion batteries and its preparation method. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of limitations of traditional sodium ion battery positive electrode materials in terms of energy density, cycle stability and cost. The present invention provides a sodium ion battery high entropy Prussian blue positive electrode material and a preparation method thereof.
[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0006] The invention discloses a sodium ion battery high entropy Prussian blue positive electrode material. The sodium ion battery high entropy Prussian blue positive electrode material is processed by the following raw materials according to the stoichiometric ratio. The stoichiometric ratio of the raw materials is as follows: sodium ferrocyanide (Na4Fe(CN)6): 20%-30%, sodium citrate (C6H5Na3O7): 3%-7%, sodium chloride (NaCl): 8%-12%, ferrous chloride (FeCl2·4H2O): 12%-18%, manganese chloride (MnCl2·4H2O): 5%-15%, cupric chloride (CuCl2·4H2O): 10%-20%, zinc chloride (ZnCl2·4H2O): 8%-12%, tin chloride (SnCl2·4H2O): 4%-6%, and cobalt chloride (CoCl2·4H2O): 3%-7%.
[0007] Furthermore, the raw materials of the high-entropy Prussian blue positive electrode material of the sodium ion battery are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 20%, sodium citrate (C6H5Na3O7): 3%, sodium chloride (NaCl): 8%, ferrous chloride (FeCl2·4H2O): 18%, manganese chloride (MnCl2·4H2O): 15%, cupric chloride (CuCl2·4H2O): 15%, zinc chloride (ZnCl2·4H2O): 12%, tin chloride (SnCl2·4H2O): 4%, and cobalt chloride (CoCl2·4H2O): 5%.
[0008] Furthermore, the raw materials of the high entropy Prussian blue positive electrode material of the sodium ion battery are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 25%, sodium citrate (C6H5Na3O7): 5%, sodium chloride (NaCl): 10%, ferrous chloride (FeCl2·4H2O): 15%, manganese chloride (MnCl2·4H2O): 10%, cupric chloride (CuCl2·4H2O): 15%, zinc chloride (ZnCl2·4H2O): 10%, tin chloride (SnCl2·4H2O): 5%, and cobalt chloride (CoCl2·4H2O): 5%.
[0009] Furthermore, the raw materials of the sodium ion battery high entropy Prussian blue positive electrode material are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 30%, sodium citrate (C6H5Na3O7): 7%, sodium chloride (NaCl): 12%, ferrous chloride (FeCl2·4H2O): 12%, manganese chloride (MnCl2·4H2O): 8%, cupric chloride (CuCl2·4H2O): 10%, zinc chloride (ZnCl2·4H2O): 8%, tin chloride (SnCl2·4H2O): 6%, and cobalt chloride (CoCl2·4H2O): 7%.
[0010] The above-mentioned method for preparing a high-entropy Prussian blue positive electrode material for a sodium ion battery comprises the following steps:
[0011] Step 1, prepare the raw materials, use an accurate electronic balance, and weigh them according to the chemical stoichiometric ratio required by the experiment, sodium ferrocyanide (Na4Fe(CN)6): 20%-30%, sodium citrate (C6H5Na3O7): 3%-7%, sodium chloride (NaCl): 8%-12%, ferrous chloride (FeCl2·4H2O): 12%-18%, manganese chloride (MnCl2·4H2O): 5%-15%, cupric chloride (CuCl2·4H2O): 10%-20%, zinc chloride (ZnCl2·4H2O): 8%-12%, tin chloride (SnCl2·4H2O): 4%-6%, cobalt chloride (CoCl2·4H2O): 3%-7%;
[0012] Step 2, preparing solution A and solution B, adding weighed sodium ferrocyanide and sodium citrate to an appropriate amount of deionized water, stirring at room temperature until completely dissolved to form a uniform solution A, and dissolving sodium chloride, ferrous chloride, manganese chloride, copper chloride, zinc chloride and tin chloride in deionized water according to a stoichiometric ratio to form a uniform solution B;
[0013] Step 3, mixing solutions A and B, placing solution A in a dropping funnel, and dripping solution A into solution B drop by drop under continuous stirring, at a dripping speed of 1-5 drops per second. After solution A is completely dripped into solution B, continue stirring for 20-30 minutes to ensure that the two solutions are fully mixed;
[0014] Step 4: reaction and precipitation: placing the mixed solution in an inert atmosphere of nitrogen (N2), heating the mixed solution to 80-90°C by a heating device, and maintaining the mixed solution at this temperature with continuous stirring for 10-12 hours to promote the reaction and the formation of the precipitate;
[0015] Step 5, precipitate treatment, using deionized water to wash the obtained precipitate multiple times to remove impurities and unreacted ions attached to the surface of the precipitate, and then using anhydrous ethanol to wash to further purify the precipitate and remove moisture, the washed precipitate is subjected to high-speed centrifugation to separate the precipitate and remove excess solvent, and the precipitate after centrifugation is placed in a vacuum drying oven and vacuum dried at an appropriate temperature until the moisture is completely removed to obtain a dry target high-entropy Prussian blue analog material.
[0016] Furthermore, in the steps 2 and 3, a magnetic stirrer is used for stirring during the preparation of solution A and solution B and the stirring reaction.
[0017] Furthermore, during the centrifugal treatment in step 5, the speed of the centrifugal equipment is set to 8000 rpm, the centrifugal time is 30 minutes, the temperature of the vacuum drying equipment is set to 60° C., and the vacuum degree should be controlled below -0.1 MPa.
[0018] The beneficial effects of the present invention are as follows:
[0019] 1. The present invention solves the limitations of traditional sodium-ion battery cathode materials in terms of energy density, cycle stability and cost. Prussian blue materials have an open framework structure, which provides a wide channel for the insertion and extraction of sodium ions, but their cycle stability and specific capacity are often challenged in practical applications. By introducing the concept of high entropy, that is, the uniform mixing of multiple transition metal elements, the structural stability and electrochemical properties of the material can be effectively improved, thereby significantly improving the energy density and cycle life of sodium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flow chart for preparing the high entropy Prussian blue positive electrode material for sodium ion batteries in the present invention. DETAILED DESCRIPTION
[0021] To make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0022] Embodiment 1:
[0023] The invention provides a sodium ion battery high entropy Prussian blue positive electrode material. The sodium ion battery high entropy Prussian blue positive electrode material is processed by the following raw materials according to a stoichiometric ratio. The raw materials are as follows: sodium ferrocyanide (Na4Fe(CN)6): 20%-30%, sodium citrate (C6H5Na3O7): 3%-7%, sodium chloride (NaCl): 8%-12%, ferrous chloride (FeCl2·4H2O): 12%-18%, manganese chloride (MnCl2·4H2O): 5%-15%, cupric chloride (CuCl2·4H2O): 10%-20%, zinc chloride (ZnCl2·4H2O): 8%-12%, tin chloride (SnCl2·4H2O): 4%-6%, and cobalt chloride (CoCl2·4H2O): 3%-7%.
[0024] Inductively coupled plasma atomic emission spectroscopy (ICP-AES), thermogravimetric (TG), X-ray diffraction (XRD), Raman, field emission scanning electron microscopy (FESEM), transmission electron microscopy (TEM), X-ray photoelectron spectroscopy (XPS), and nitrogen adsorption-desorption tests were used to characterize the composition, interstitial water molecules and [Fe(CN)6]4- anion defect content, structure, morphology, size, surface electronic state, specific surface area and pore structure, carbon content and other properties of the material. The formation mechanism and influencing factors of interstitial water molecules and anion vacancies were explored, and the process parameters were optimized to achieve the controllable synthesis of low-defect five-component Prussian blue analogue composites. The group classified and calculated the relationship between parameters such as etchant type and concentration, sodium source type and molar ratio with Prussian blue-based materials, etching / activation temperature and time, and surface pore structure distribution, number of surface active sites, and anion defect content. The defect-induced heterogeneous reaction process was studied to reveal the control mechanism of key parameters on surface physical properties. Through experiments and calculations, the team finally determined the high-entropy Prussian blue positive electrode material whose high-entropy components are Mn, Fe, Zn, Co, Cu, and Sn.
[0025] It solves the limitations of traditional sodium-ion battery cathode materials in terms of energy density, cycle stability and cost. Prussian blue materials have an open framework structure, which provides a wide channel for the insertion and extraction of sodium ions, but their cycle stability and specific capacity are often challenged in practical applications. By introducing the concept of high entropy, that is, the uniform mixing of multiple transition metal elements, the structural stability and electrochemical performance of the material can be effectively improved, thereby significantly improving the energy density and cycle life of sodium-ion batteries.
[0026] High-entropy Prussian blue cathode materials also bring cost advantages. The main raw materials of Prussian blue are relatively cheap compounds such as sodium cyanide, and no expensive metal elements are used, so its material cost is relatively low. At the same time, high-entropy design can further optimize the material synthesis process, reduce energy consumption and waste emissions in the production process, and meet the requirements of sustainable development.
[0027] See also Figure 1 The above-mentioned method for preparing a high entropy Prussian blue positive electrode material for a sodium ion battery comprises the following steps:
[0028] Step 1, prepare the raw materials, use an accurate electronic balance, and weigh them according to the chemical stoichiometric ratio required by the experiment, sodium ferrocyanide (Na4Fe(CN)6): 20%-30%, sodium citrate (C6H5Na3O7): 3%-7%, sodium chloride (NaCl): 8%-12%, ferrous chloride (FeCl2·4H2O): 12%-18%, manganese chloride (MnCl2·4H2O): 5%-15%, cupric chloride (CuCl2·4H2O): 10%-20%, zinc chloride (ZnCl2·4H2O): 8%-12%, tin chloride (SnCl2·4H2O): 4%-6%, cobalt chloride (CoCl2·4H2O): 3%-7%;
[0029] Step 2, preparing solution A and solution B, adding weighed sodium ferrocyanide and sodium citrate to an appropriate amount of deionized water, stirring at room temperature until completely dissolved to form a uniform solution A, and dissolving sodium chloride, ferrous chloride, manganese chloride, copper chloride, zinc chloride and tin chloride in deionized water according to a stoichiometric ratio to form a uniform solution B;
[0030] Step 3, mixing solutions A and B, placing solution A in a dropping funnel, and dripping solution A into solution B drop by drop under continuous stirring, at a dripping speed of 1-5 drops per second. After solution A is completely dripped into solution B, continue stirring for 20-30 minutes to ensure that the two solutions are fully mixed;
[0031] Step 4: reaction and precipitation: placing the mixed solution in an inert atmosphere of nitrogen (N2), heating the mixed solution to 80-90°C by a heating device, and maintaining the mixed solution at this temperature with continuous stirring for 10-12 hours to promote the reaction and the formation of the precipitate;
[0032] Step 5, precipitate treatment, using deionized water to wash the obtained precipitate multiple times to remove impurities and unreacted ions attached to the surface of the precipitate, and then using anhydrous ethanol to wash to further purify the precipitate and remove moisture, the washed precipitate is subjected to high-speed centrifugation to separate the precipitate and remove excess solvent, and the precipitate after centrifugation is placed in a vacuum drying oven and vacuum dried at an appropriate temperature until the moisture is completely removed to obtain a dry target high-entropy Prussian blue analog material.
[0033] In this embodiment, preferably, a magnetic stirrer is used for stirring processing when preparing solution A and solution B and stirring the reaction in step 2 and step 3.
[0034] In this embodiment, preferably, during the centrifugal treatment in step 5, the speed of the centrifugal device is set to 8000 rpm, the centrifugal time is 30 minutes, the temperature of the vacuum drying device is set to 60° C., and the vacuum degree should be controlled below -0.1 MPa.
[0035] Embodiment 2:
[0036] In this embodiment, preferably, the raw materials of the high entropy Prussian blue positive electrode material of the sodium ion battery are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 20%, sodium citrate (C6H5Na3O7): 3%, sodium chloride (NaCl): 8%, ferrous chloride (FeCl2·4H2O): 18%, manganese chloride (MnCl2·4H2O): 15%, cupric chloride (CuCl2·4H2O): 15%, zinc chloride (ZnCl2·4H2O): 12%, tin chloride (SnCl2·4H2O): 4%, and cobalt chloride (CoCl2·4H2O): 5%.
[0037] Embodiment 3:
[0038] In this embodiment, preferably, the raw materials of the sodium ion battery high entropy Prussian blue positive electrode material are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 25%, sodium citrate (C6H5Na3O7): 5%, sodium chloride (NaCl): 10%, ferrous chloride (FeCl2·4H2O): 15%, manganese chloride (MnCl2·4H2O): 10%, cupric chloride (CuCl 2·4H2O): 15%, zinc chloride (ZnCl 2·4H2O): 10%, tin chloride (SnCl2·4H2O): 5%, and cobalt chloride (CoCl2·4H2O): 5%.
[0039] Embodiment 4:
[0040] In this embodiment, preferably, the raw materials of the sodium ion battery high entropy Prussian blue positive electrode material are in a stoichiometric ratio of sodium ferrocyanide (Na4Fe(CN)6): 30%, sodium citrate (C6H5Na3O7): 7%, sodium chloride (NaCl): 12%, ferrous chloride (FeCl2·4H2O): 12%, manganese chloride (MnCl2·4H2O): 8%, cupric chloride (CuCl2·4H2O): 10%, zinc chloride (ZnCl2·4H2O): 8%, tin chloride (SnCl2·4H2O): 6%, and cobalt chloride (CoC l 2·4H2O): 7%.
[0041] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high entropy Prussian blue cathode material for sodium ion batteries, Features: The high entropy Prussian blue positive electrode material for sodium ion batteries is prepared by processing the following raw materials according to a stoichiometric ratio, wherein the raw materials are processed according to a stoichiometric ratio of sodium ferrocyanide (Na 4 Fe(CN) 6 ): 20% to 30%, sodium citrate (C 6 H 5 Na 3 O 7 ): 3% to 7%, sodium chloride (NaCl): 8% to 12%, ferrous chloride (FeCl 2 ·4H 2 O): 12% to 18%, manganese chloride (MnCl 2 ·4H 2 O): 5% to 15%, copper chloride (CuCl 2 ·4H 2 O): 10% to 20%, zinc chloride (ZnCl 2 ·4H 2 O): 8% to 12%, tin chloride (SnCl 2 ·4H 2 O): 4% to 6%, cobalt chloride (CoCl 2 ·4H 2 O): 3% to 7%.
2. A sodium ion battery high entropy Prussian blue positive electrode material according to claim 1, Features: The raw materials of the high entropy Prussian blue positive electrode material of the sodium ion battery are in the following stoichiometric ratio: sodium ferrocyanide (Na 4 Fe(CN) 6 ): 20%, sodium citrate (C 6 H 5 Na 3 O 7 ): 3%, sodium chloride (NaCl): 8%, ferrous chloride (FeCl 2 ·4H 2 O): 18%, manganese chloride (MnCl 2 ·4H 2 O): 15%, copper chloride (CuCl 2 ·4H 2 O): 15%, zinc chloride (ZnCl 2 ·4H 2 O): 12%, tin chloride (SnCl 2 ·4H 2 O): 4%, cobalt chloride (CoCl 2 ·4H 2 O): 5%.
3. A sodium ion battery high entropy Prussian blue positive electrode material according to claim 1, Features: The raw materials of the high entropy Prussian blue positive electrode material of the sodium ion battery are in the following stoichiometric ratio: sodium ferrocyanide (Na 4 Fe(CN) 6 ): 25%, sodium citrate (C 6 H 5 Na 3 O 7 ):5%、Sodium chloride (NaCl):10%、Ferrous chloride (FeCl 2 ·4H 2 O): 15%, manganese chloride (MnCl 2 ·4H 2 O): 10%, copper chloride (CuCl 2 ·4H 2 O): 15%, zinc chloride (ZnCl 2 ·4H 2 O): 10%, tin chloride (SnCl 2 ·4H 2 O): 5%, cobalt chloride (CoCl 2 ·4H 2 O): 5%.
4. A sodium ion battery high entropy Prussian blue positive electrode material according to claim 1, Features: The raw materials of the high entropy Prussian blue positive electrode material of the sodium ion battery are in the following stoichiometric ratio: sodium ferrocyanide (Na 4 Fe(CN) 6 ): 30%, sodium citrate (C 6 H 5 Na 3 O 7 ): 7%, sodium chloride (NaCl): 12%, ferrous chloride (FeCl 2 ·4H 2 O): 12%, manganese chloride (MnCl 2 ·4H 2 O): 8%, copper chloride (CuCl 2 ·4H 2 O): 10%, zinc chloride (ZnCl 2 ·4H 2 O): 8%, tin chloride (SnCl 2 ·4H 2 O): 6%, cobalt chloride (CoCl 2 ·4H 2 O): 7%.
5. A method for preparing a high entropy Prussian blue cathode material for a sodium ion battery. It is characterized in that It includes the following steps: Step 1: Prepare the raw materials. Use an accurate electronic balance to weigh the sodium ferrocyanide (Na 4 Fe(CN) 6 ): 20% to 30%, sodium citrate (C 6 H 5 Na 3 O 7 ): 3% to 7%, sodium chloride (NaCl): 8% to 12%, ferrous chloride (FeCl 2 ·4H 2 O): 12% to 18%, manganese chloride (MnCl 2 ·4H 2 O): 5% to 15%, copper chloride (CuCl 2 ·4H 2 O): 10% to 20%, zinc chloride (ZnCl 2 ·4H 2 O): 8% to 12%, tin chloride (SnCl 2 ·4H 2 O): 4% to 6%, cobalt chloride (CoCl 2 ·4H 2 O): 3% to 7%; Step 2, preparing solution A and solution B, adding weighed sodium ferrocyanide and sodium citrate to an appropriate amount of deionized water, stirring at room temperature until completely dissolved to form a uniform solution A, and dissolving sodium chloride, ferrous chloride, manganese chloride, copper chloride, zinc chloride and tin chloride in deionized water according to a stoichiometric ratio to form a uniform solution B; Step 3, mixing solutions A and B, placing solution A in a dropping funnel, and dripping solution A into solution B drop by drop under continuous stirring, at a dripping speed of 1-5 drops per second. After solution A is completely dripped into solution B, continue stirring for 20-30 minutes to ensure that the two solutions are fully mixed; Step 4: reaction and precipitation: placing the mixed solution in an inert atmosphere of nitrogen (N2), heating the mixed solution to 80-90°C by a heating device, and maintaining the mixed solution at this temperature with continuous stirring for 10-12 hours to promote the reaction and the formation of the precipitate; Step 5, precipitate treatment, using deionized water to wash the obtained precipitate multiple times to remove impurities and unreacted ions attached to the surface of the precipitate, and then using anhydrous ethanol to wash to further purify the precipitate and remove moisture, the washed precipitate is subjected to high-speed centrifugation to separate the precipitate and remove excess solvent, and the precipitate after centrifugation is placed in a vacuum drying oven and vacuum dried at an appropriate temperature until the moisture is completely removed to obtain a dry target high-entropy Prussian blue analog material.
6. A method for preparing a high entropy Prussian blue positive electrode material for a sodium ion battery according to claim 5, Features: In the steps 2 and 3, a magnetic stirrer is used for stirring during the preparation of solution A and solution B and the stirring reaction.
7. The method for preparing a high entropy Prussian blue positive electrode material for a sodium ion battery according to claim 5, Features: During the centrifugal treatment in step 5, the speed of the centrifugal device is set to 8000 rpm, the centrifugal time is 30 minutes, the temperature of the vacuum drying device is set to 60° C., and the vacuum degree should be controlled below -0.1 MPa.
Citation Information
Patent Citations
High-entropy Prussian blue material and preparation method thereof
CN113690433A
Sodium-ion battery positive electrode material as well as preparation method and application thereof
CN116443894A
High-entropy Prussian blue-based positive electrode material of sodium ion battery and preparation method of high-entropy Prussian blue-based positive electrode material
CN116768236A
Universal method for ultrafast preparation of sodium ion battery layered oxide positive electrode material based on Prussian blue analogue and application
CN117747797A
Preparation method of high-entropy oxide and positive electrode material
CN118005090A
Cited By
Preparation method and application of high-entropy Prussian blue positive electrode material
CN120646863A