Method for recovering lithium in waste lithium ion battery
By mixing the black powder from used lithium-ion batteries with alkali materials and roasting them under aerobic conditions, combined with leaching and crystallization treatments, the problem of low purity of lithium-containing products in lithium-ion battery recycling has been solved, and efficient and low-cost recycling has been achieved. Lithium ion recycling.
Patent Information
- Application Number
- CN202410730902.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-11
AI Technical Summary
The purity of lithium-containing products after lithium recovery from used lithium-ion batteries is low, and existing recycling technologies are costly and inefficient.
The roasted raw meal is obtained by mixing the black powder from used lithium-ion batteries with alkali materials, roasting it under aerobic conditions, and then mixing it with a leaching agent for leaching treatment. Finally, a high-purity lithium salt is obtained through crystallization treatment.
It effectively improves the purity of the recycled lithium salt, reduces process costs, and achieves efficient recovery of lithium from used lithium-ion batteries.
Smart Images

Figure CN118754162A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium ion battery recycling, and in particular to a method for recycling lithium in waste lithium ion batteries. Background Art
[0002] Lithium-ion battery is a rechargeable chemical battery with good comprehensive performance. It has the advantages of high operating voltage, high specific energy, long cycle life, and low self-discharge. It is widely used in mobile communications, laptop batteries, portable tools, electric vehicles and other fields. The positive electrode materials used in lithium-ion secondary batteries on the market are mainly lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and other binary / ternary materials containing lithium. These positive electrode materials all contain precious metallic lithium resources. Since lithium-ion batteries use a large amount of positive electrode materials, the consumption of non-renewable metal resources is very large. Therefore, while the use of lithium-ion batteries is increasing day by day, the recovery of high-value and high-content metals in waste lithium-ion batteries is of great significance to achieving energy conservation, emission reduction and sustainable development.
[0003] Although the commercialization technology of lithium-ion batteries has become increasingly mature over the past few decades, the research and development of the corresponding waste lithium-ion battery recycling technology is relatively lagging behind, especially the low purity of the lithium-containing products obtained after a series of complex chemical treatments.
[0004] The above contents are only used to assist in understanding the technical solution of the present application and do not constitute an admission that the above contents are prior art. Summary of the invention
[0005] The main purpose of the present application is to provide a method for recovering lithium from waste lithium-ion batteries, aiming to solve the technical problem of low purity of lithium-containing products after lithium recovery from waste lithium-ion batteries.
[0006] To achieve the above object, the present application proposes a method for recovering lithium from waste lithium-ion batteries, the method comprising:
[0007] Obtain black powder from used lithium-ion batteries;
[0008] The black powder is mixed with an alkali material to obtain a roasted raw meal;
[0009] Roasting the roasted raw material under aerobic conditions to obtain roasted clinker;
[0010] The roasted clinker is mixed with a leaching agent for leaching to obtain a lithium-containing leaching solution;
[0011] The lithium-containing leaching solution is crystallized to obtain lithium salt.
[0012] In one embodiment, the mass ratio between the black powder and the alkali material is 1:(0.5-3);
[0013] And / or, the alkali material comprises: at least one of sodium hydroxide, potassium hydroxide, calcium oxide, calcium hydroxide, magnesium hydroxide and magnesium oxide;
[0014] And / or, the particle size of the black powder is 100-200 meshes.
[0015] In one embodiment, the step of roasting the raw material under aerobic conditions to obtain roasted clinker comprises:
[0016] Pressing the roasted raw material into spherical raw material with a particle size of 4 to 20 mm;
[0017] The spherical raw material is roasted under aerobic conditions to obtain the roasted clinker.
[0018] In one embodiment, the calcination temperature is 500-1000° C., and the calcination time is 0.5-12 hours.
[0019] In one embodiment, the leaching temperature of the leaching treatment is 60-100° C., and the leaching time is 1-5 hours;
[0020] And / or, the solid-to-liquid ratio between the roasted clinker and the leaching agent is 1:(3-30).
[0021] In one embodiment, the step of crystallizing the lithium-containing leachate to obtain a lithium salt comprises:
[0022] The lithium-containing leaching solution is sequentially passed through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin to remove impurities, thereby obtaining a lithium-containing impurity-removed solution;
[0023] The lithium-containing impurity-removing liquid is subjected to crystallization treatment to obtain the lithium salt.
[0024] In one embodiment, the step of crystallizing the lithium-containing leachate to obtain a lithium salt comprises:
[0025] Passing the lithium-containing leaching solution into a bipolar membrane system to obtain a lithium hydroxide solution;
[0026] The lithium hydroxide solution is subjected to crystallization treatment to obtain lithium hydroxide.
[0027] In one embodiment, the acid solution produced by the bipolar membrane system is used to prepare the leaching agent.
[0028] In one embodiment, the step of crystallizing the lithium-containing leachate to obtain a lithium salt comprises:
[0029] The lithium-containing leachate is subjected to reverse osmosis concentration to obtain a lithium-containing concentrated solution and a permeate;
[0030] The lithium-containing concentrated solution is evaporated and crystallized to obtain the lithium salt and condensed water, wherein the condensed water and the permeate are used to prepare the leaching agent.
[0031] In one embodiment, the step of mixing the black powder with an alkali material to obtain a roasted raw material comprises:
[0032] The black powder and the alkali material are mixed and ground for 0.5 to 3 hours to obtain the roasted raw material.
[0033] One or more technical solutions proposed in this application have at least the following technical effects: obtaining black powder from waste lithium-ion batteries; then mixing the black powder with an alkali material to obtain a roasted raw material; then roasting the roasted raw material under aerobic conditions to obtain a roasted clinker; then mixing the roasted clinker with a leaching agent for leaching treatment to obtain a lithium-containing leachate; then crystallizing the lithium-containing leachate to obtain a lithium salt. Since an alkali material is added to the black powder before leaching, the impurities (for example, aluminum, iron, phosphate, etc.) in the black powder other than lithium are fixed by the alkali material, so that each impurity forms an insoluble substance, which effectively improves the purity of the recovered lithium salt. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0036] Figure 1 A schematic diagram of a process for recovering lithium from waste lithium-ion batteries provided in Example 1 of the present application;
[0037] Figure 2 This is a flow chart of a relatively complete embodiment of the method for recovering lithium from waste lithium-ion batteries of the present application.
[0038] The purpose, features and advantages of this application will be further described in conjunction with the embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] Hereinafter, the embodiments of the method for recovering lithium from waste lithium-ion batteries of the present application will be described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually identical structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the accompanying drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0041] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0042] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0043] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0044] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0045] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0046] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0047] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and understandable, the technical solution of the present application is further described below in conjunction with the accompanying drawings and embodiments. However, the present application is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed in the present application.
[0048] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present application. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0049] In order to better understand the technical solution of the present application, a detailed description will be given below in conjunction with the accompanying drawings and specific implementation methods.
[0050] Among conventional technologies, the recycling of waste lithium-ion batteries currently mainly involves wet processes, which have low equipment requirements, simple processes, easy operations, and relatively high metal recovery rates. However, high recovery rates rely on the addition of strong acids, strong bases, and strong reducing agents, which consume a huge amount of material and result in high process costs. At the same time, the purity of the lithium-containing products obtained after recycling is low.
[0051] The present application provides a solution, by obtaining black powder from waste lithium-ion batteries; then mixing the black powder with an alkali material to obtain a roasted raw material; then roasting the roasted raw material under aerobic conditions to obtain a roasted clinker; then mixing the roasted clinker with a leaching agent for leaching treatment to obtain a lithium-containing leachate; then crystallizing the lithium-containing leachate to obtain a lithium salt. Since an alkali material is added to the black powder before leaching, the impurities (for example, aluminum, iron, phosphate, etc.) in the black powder other than lithium are fixed by the alkali material, so that each impurity forms an insoluble substance, which effectively improves the purity of the recovered product lithium salt.
[0052] Based on this, the present application embodiment provides a method for recovering lithium from waste lithium-ion batteries. Figure 1 , Figure 1 The flowchart of the first embodiment of the method for recovering lithium from waste lithium-ion batteries of the present application is shown in FIG. In this embodiment, the method for recovering lithium from waste lithium-ion batteries comprises:
[0053] Step S10, obtaining black powder from waste lithium-ion batteries;
[0054] In a feasible embodiment, black powder is obtained from waste lithium-ion batteries, wherein the black powder can be a mixed powder containing positive electrode materials and negative electrode materials obtained by crushing, grinding, sieving and other steps of the waste lithium-ion batteries.
[0055] Optionally, waste lithium-ion batteries are obtained and cut, crushed, and processed through a crusher to separate the battery shell, electrolyte, positive and negative electrodes; the crushed lithium battery material is then put into a grinder for grinding, thereby grinding the metal shell of the lithium battery into small particles for subsequent sorting and recycling; the ground lithium battery material is then sieved through a disc screen to collect black powder.
[0056] Optionally, the waste lithium-ion batteries may include: lithium iron phosphate batteries, lithium cobalt oxide batteries, lithium manganese oxide batteries, nickel cobalt manganese oxide batteries, etc.
[0057] In a feasible implementation, the particle size of the black powder is 100-200 mesh; for example, the particle size of the black powder is 100 mesh, 110 mesh, 120 mesh, 130 mesh, 140 mesh, 150 mesh, 160 mesh, 170 mesh, 180 mesh, 190 mesh, 200 mesh, etc. If the particle size of the black powder is too large, it may lead to insufficient contact between the black powder and the alkali material, affecting the reaction efficiency; and by pre-screening the size of the black powder, subsequent processing (for example, grinding) time can be saved; therefore, the particle size of the black powder is determined to be 100-200 mesh.
[0058] Step S20, mixing the black powder with an alkali material to obtain a roasted raw material;
[0059] In a feasible embodiment, black powder is mixed with an alkali material to obtain a roasted raw meal.
[0060] Optionally, the mass ratio between the black powder and the alkali material in the roasted raw material is 1:(0.5-3); for example, the mass ratio between the black powder and the alkali material in the roasted raw material is 1:0.5, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8, 1:3, etc. Since the alkali material is mainly used for impurities such as aluminum, iron, and phosphate in the black powder, if the amount of alkali material added is too low, some impurities may be dissolved in the leachate together with the formed lithium carbonate, and affect the purity of the final recovered product; and if the amount of alkali added is too large, it is difficult to further improve the purity of the product, but increase the process cost. Therefore, it is determined that the mass ratio between the black powder and the alkali material in the roasted raw material is 1:(0.5-3).
[0061] Optionally, the alkali material includes at least one of sodium hydroxide, potassium hydroxide, calcium oxide, calcium hydroxide, magnesium hydroxide and magnesium oxide.
[0062] Optionally, the alkali material includes: calcium oxide, calcium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide and magnesium oxide, and the mass ratio between the components is (3-15):(0.01-10):(0.01-0.9):(0.01-0.6):(0.01-9):(0.01-13). By mixing a variety of alkali materials, the alkalinity of the alkali material can be effectively improved, the fixation effect on impurities such as aluminum, iron, phosphate in the black powder can be enhanced, and the purity of the product can be improved.
[0063] In one feasible implementation, step S20, mixing the black powder with an alkali material to obtain a roasted raw material comprises:
[0064] Step S21, mixing the black powder and the alkali material and grinding them for 0.5 to 3 hours to obtain the roasted raw material.
[0065] In a feasible embodiment, the black powder and the alkali material are mixed and ground for a grinding time of 0.5 to 3 hours to obtain the roasted raw meal.
[0066] In this embodiment, grinding can make the particles of the roasted raw material finer, and smaller particles are more easily affected by heat, thereby increasing the subsequent reaction rate; at the same time, grinding can also make the black powder and the alkali material mixed more evenly, avoiding the situation where the concentration of the alkali material is too high or too low locally, which helps to maintain stable reaction conditions during the roasting process. The grinding time can be: 0.5h, 0.8h, 1.2h, 1.6h, 2h, 2.4h, 2.8h, 2.9h, 3h, etc. If the grinding time is too short, the material particles may not be fully refined, resulting in insufficient contact area between particles, affecting the reaction efficiency and uniformity between materials during the roasting process; at the same time, larger particles may cause insufficient reaction during the roasting process, resulting in a reduction in the amount of target product generated or a reduction in the generation rate; in addition, due to the larger particles, higher temperatures and longer times may be required during roasting to achieve the desired degree of reaction, which will increase energy consumption and production costs. If the grinding time is too long, more energy and time will be consumed, resulting in an increase in production costs. At the same time, long-term grinding may cause changes in material properties, such as changes in crystal structure or loss of active components, thereby affecting the effect of the subsequent roasting process. Therefore, the grinding time is determined to be 0.5 to 3 hours.
[0067] Step S30, roasting the raw material under aerobic conditions to obtain roasted clinker;
[0068] In a feasible embodiment, the raw material is roasted under oxygen conditions to obtain roasted clinker.
[0069] Optionally, the roasting is high-temperature roasting, and the roasting temperature is 500-1000°C; for example, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, etc. If the roasting temperature is too low, the roasted clinker may not be roasted thoroughly, resulting in less lithium carbonate formation, which ultimately affects the leaching rate and recovery rate of lithium; at the same time, the impurity aluminum contained in the roasted clinker may be dissolved in the leachate together with the lithium carbonate produced after roasting during the leaching process, resulting in the purity of the final product being affected. If the roasting temperature is too high, the crystal structure of lithium in the black powder may be destroyed, making the release of lithium ions more difficult, which in turn affects the formation of lithium carbonate and the leaching rate and recovery rate of lithium. Therefore, as the roasting temperature increases, the leaching rate and recovery rate of lithium will first increase and then decrease.
[0070] Optionally, the calcination time is 0.5 to 12 hours, for example, 0.5 hours, 1 hour, 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, etc. The calcination time may be the holding time after the temperature is raised to 500 to 1000°C.
[0071] Alternatively, low-temperature roasting can be achieved by microwave heating; microwave heating relies on microwave electromagnetic field heating, which is achieved by high-frequency reciprocating motion of dipole molecules inside the heated body, generating "internal friction heat" to heat the material inside and outside at the same time, with fast and uniform heating speed, and only a few or a few tenths of the energy consumption of conventional heating methods can be used to achieve the heating purpose. At the same time, microwave heating can selectively heat polar molecules, and lithium iron phosphate is a polar molecule; therefore, microwave heating generates thermal stress, thereby selectively destroying the interlayer structure of lithium and oxygen, increasing the contact area, and thus achieving efficient lithium recovery at lower temperatures. Under microwave heating conditions, the calcination temperature can be 200-500°C, for example, the calcination temperature is 200°C, 220°C, 240°C, 250°C, 260°C, 280°C, 300°C, 320°C, 340°C, 350°C, 360°C, 380°C, 400°C, 420°C, 440°C, 450°C, 460°C, 480°C, 500°C, etc.
[0072] Optionally, the roasted raw material is placed in an alkalization rotary kiln and air and / or oxygen are introduced for roasting. The alkalization rotary kiln changes the alkali decomposition reaction from a traditional solid-liquid reaction to a solid-solid reaction, thereby achieving continuous productivity of alkali roasting.
[0073] In one feasible implementation, step S30, roasting the raw material under aerobic conditions to obtain roasted clinker comprises:
[0074] Step S31, pressing the roasted raw material into spherical raw material with a particle size of 4 to 20 mm;
[0075] Step S32, roasting the spherical raw material under aerobic conditions to obtain the roasted clinker.
[0076] In a feasible embodiment, the roasted raw material is pressed into spherical raw material with a particle size of 4 to 20 mm, and then the spherical raw material is roasted under aerobic conditions to obtain the roasted clinker. The particle size of the spherical raw material can be 4 mm, 6 mm, 8 mm, 10 mm, 12 mm, 14 mm, 16 mm, 17 mm, 18 mm, 19 mm, 20 mm, etc.
[0077] In this embodiment, since the particle size and density of each component in the roasted raw material may be different, which may easily lead to segregation during the subsequent roasting process, this embodiment uses granulation to make each component stick together tightly, effectively preventing the occurrence of segregation, thereby ensuring the stability of the proportion of each component during the roasting process; it can also increase the contact area of the reactants (i.e., roasted clinker) and improve the reaction efficiency. Furthermore, if the particle size of the spherical raw material is too small, it may re-agglomerate due to the increase in surface energy, resulting in poor fluidity; at the same time, during the roasting process, the particles with too small a particle size may react too fast, resulting in local overheating or uneven reaction. If the particle size is too large, the reaction speed is slow during the roasting process, and a higher temperature and longer time may be required to achieve the desired degree of reaction; therefore, it is determined to produce a spherical raw material with a particle size of 4 to 20 mm.
[0078] Step S40, mixing the roasted clinker with a leaching agent for leaching treatment to obtain a lithium-containing leaching solution;
[0079] In a feasible embodiment, the roasted clinker is mixed with a leaching agent for leaching treatment, and after leaching, the solid-liquid separation is performed to collect the lithium-containing leachate.
[0080] Optionally, the leaching solution may be a solution of sulfuric acid, hydrochloric acid or phosphoric acid.
[0081] Optionally, the leaching temperature of the leaching treatment is 60-100°C; for example, the leaching temperature is 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.
[0082] Optionally, the leaching time is 1 to 5 h; for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, etc.
[0083] Optionally, the solid-liquid ratio between the roasted clinker and the leaching agent is 1:(3-20); for example, the solid-liquid ratio between the roasted clinker and the leaching agent is 1:3, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, 1:22, 1:24, 1:26, 1:28, 1:30, etc. If the amount of leaching agent added is low, it is difficult to fully react with the roasted clinker, affecting the leaching efficiency of lithium in the roasted clinker; and if the amount of leaching agent added is too high, it is difficult to further improve the leaching efficiency of lithium in the roasted clinker, and the required production cost is higher; therefore, the solid-liquid ratio between the roasted clinker and the leaching agent is determined to be 1:(3-20).
[0084] Step S50, performing crystallization treatment on the lithium-containing leaching solution to obtain lithium salt.
[0085] In a feasible embodiment, the lithium-containing leaching solution is crystallized to obtain lithium salt, thereby achieving high-purity recovery of lithium in waste lithium-ion batteries.
[0086] In one feasible implementation, step S50, the step of crystallizing the lithium-containing leaching solution to obtain a lithium salt comprises:
[0087] Step S51, removing impurities from the lithium-containing leaching solution by sequentially passing through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin to obtain a lithium-containing impurity-removed solution;
[0088] Step S52, performing crystallization treatment on the lithium-containing impurity-removing liquid to obtain the lithium salt.
[0089] In a feasible embodiment, since an alkali material is used for mixed low-temperature roasting, the lithium-containing leachate may also contain impurities such as calcium, magnesium, sodium, and potassium. In order to improve the purity of the lithium salt, the lithium-containing leachate is sequentially passed through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin for impurity removal, wherein the hydrogen-type cation exchange resin may be a 732-type strong acid cation exchange resin, which is used to remove sodium, potassium ions, calcium and magnesium ions, etc. from the lithium-containing leachate, and the strong alkaline ion exchange resin is used to remove free aluminate from the lithium-containing leachate to obtain a lithium-containing impurity-removed liquid, and then the lithium-containing impurity-removed liquid is crystallized to obtain the lithium salt.
[0090] In this embodiment, the calcium, magnesium, sodium and / or potassium ion impurities introduced into the lithium-containing leachate due to the alkali material are effectively filtered out based on the hydrogen type cation exchange resin and the strong alkaline ion exchange resin, thereby improving the purity of the final product (lithium salt).
[0091] In one feasible implementation, step S50, the step of crystallizing the lithium-containing leaching solution to obtain a lithium salt comprises:
[0092] Step S53, passing the lithium-containing leaching solution into a bipolar membrane system to obtain a lithium hydroxide solution;
[0093] Step S54, performing crystallization treatment on the lithium hydroxide solution to obtain lithium hydroxide.
[0094] In one feasible embodiment, the lithium-containing leaching solution is passed into a bipolar membrane system, which is mainly composed of a cation exchange layer, an interface catalyst layer and an anion exchange layer. Under the action of a DC electric field, water in the bipolar membrane system is dissociated into H + and OH - , and migrate to both sides of the membrane through the cation membrane and the anion membrane respectively, realizing the separation of cations and anions. The reaction formula of the chemical reaction that occurs when the roasted clinker is leached with the leaching agent can be:
[0095] Li2CO3+H2SO4=Li2SO4+H2O+CO2↑
[0096] That is, the generated lithium-containing leaching solution contains lithium sulfate, and then the lithium sulfate solution is passed into the bipolar membrane system to react with the OH generated in the bipolar membrane system. - The reaction generates lithium hydroxide, that is, a lithium hydroxide solution. At the same time, the bipolar membrane system can also produce an acid solution, such as sulfuric acid; the acid solution produced by the bipolar membrane system can be reused to prepare a leaching agent, and can also be used to regenerate hydrogen-type cation exchange resins and strong alkaline ion exchange resins, thereby realizing resource recycling and reducing process costs.
[0097] It should be understood that if the leaching agent is phosphoric acid or hydrochloric acid, the lithium-containing leachate may contain lithium phosphate, lithium chloride, etc.; accordingly, after the lithium-containing leachate is passed into the bipolar membrane system, the acid solution generated by the bipolar membrane system may be a phosphoric acid solution, a hydrochloric acid solution, etc.
[0098] Optionally, the lithium-containing leachate is sequentially passed through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin to remove impurities to obtain a lithium-containing impurity-removed liquid; the lithium-containing impurity-removed liquid is passed through a bipolar membrane system to obtain a lithium hydroxide solution; and the lithium hydroxide solution is crystallized to obtain lithium hydroxide.
[0099] In one feasible implementation, step S50, the step of crystallizing the lithium-containing leaching solution to obtain a lithium salt comprises:
[0100] Step S55, performing reverse osmosis concentration on the lithium-containing leachate to obtain a lithium-containing concentrated solution and a permeate;
[0101] Step S56, evaporating and crystallizing the lithium-containing concentrated solution to obtain the lithium salt and condensed water, wherein the condensed water and the permeate are used to prepare the leaching agent.
[0102] In a feasible embodiment, the lithium-containing leachate is subjected to reverse osmosis concentration to obtain a lithium-containing concentrated solution and a permeate, and then the lithium-containing concentrated solution is evaporated and crystallized to obtain the lithium salt and condensed water; the condensed water and the permeate generated during the concentration and crystallization process can be used to prepare a leaching agent; for example, the condensed water and the permeate are mixed with the original leaching agent and used as a new leaching agent to achieve resource recycling.
[0103] To assist in understanding the above technical solution, a relatively complete embodiment of a method for recovering lithium from waste lithium-ion batteries is described below. Figure 2, obtaining waste lithium-ion batteries and collecting black powder through steps such as crushing; mixing the black powder with an alkali material to obtain a roasted raw material, and roasting the roasted raw material at a low temperature in an oxygen environment to obtain a roasted clinker; mixing the roasted clinker with a leaching agent for leaching treatment to obtain a lithium-containing leachate; removing impurities from the lithium-containing leachate by passing it through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin in sequence to obtain a lithium-containing impurity-removed liquid; passing the lithium-containing impurity-removed liquid into a bipolar membrane system to obtain a lithium hydroxide solution and an acid solution, wherein the acid solution is used to configure the leaching agent; then passing the lithium hydroxide solution into an RO (reverse osmosis) module for reverse osmosis concentration to obtain a lithium hydroxide concentrate and a permeate, passing the lithium hydroxide concentrate into an MVR (steam mechanical recompression technology, Mechanical Vapor Recompression) for evaporation and crystallization to obtain lithium hydroxide and condensed water; and the obtained condensed water and the permeate can be used to configure the leaching agent and return to the process flow for leaching.
[0104] In this embodiment, black powder is obtained from waste lithium-ion batteries; the black powder is mixed with an alkali material to obtain a roasted raw material; the roasted raw material is roasted under aerobic conditions to obtain a roasted clinker; the roasted clinker is mixed with a leaching agent for leaching treatment to obtain a lithium-containing leachate; the lithium-containing leachate is crystallized to obtain a lithium salt. Since an alkali material is added to the black powder before leaching, the impurities (for example, aluminum, iron, phosphate, etc.) other than lithium in the black powder are fixed by the alkali material, so that each impurity becomes insoluble, which effectively improves the purity of the lithium salt of the recovered product; and after the lithium-containing leachate is obtained by leaching, the lithium-containing leachate is successively passed through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin for impurity removal, so as to further improve the purity of the product; and then the lithium-containing leachate is passed through a bipolar membrane system to obtain a lithium hydroxide solution, and a lithium hydroxide product is obtained by crystallization, so as to realize the efficient recovery of lithium in waste lithium-ion batteries; at the same time, the acid solution generated in the bipolar membrane system during the recovery process, and the permeate and condensed water generated in the reverse osmosis concentration and evaporative crystallization can be reused to configure the leaching agent, so as to realize the recycling of resources and effectively reduce the process cost.
[0105] In order to enable the details and operations of the above embodiments of the present application to be clearly understood by those skilled in the art, and to demonstrate the significant improvement in the performance of the method for recovering lithium from waste lithium-ion batteries in the embodiments of the present application, the above technical scheme is illustrated by means of multiple embodiments below.
[0106] Example 1
[0107] (1) Obtaining black powder from waste lithium-ion batteries;
[0108] (2) mixing black powder and calcium oxide in a mass ratio of 1:1 and grinding for 2 hours to obtain a roasted raw meal;
[0109] (3) feeding the roasted raw material into an alkaline rotary kiln, keeping the temperature at 800° C. for 4 h, cooling and taking it out to obtain roasted clinker;
[0110] (4) mixing the roasted clinker and the leaching agent at a solid-liquid mass ratio of 1:5, and leaching at 80° C. for 1 hour to obtain a lithium-containing leaching solution, wherein the leaching agent includes: sulfuric acid;
[0111] (5) removing impurities from the lithium-containing leaching solution by sequentially passing through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin to obtain a lithium-containing impurity-removed solution;
[0112] (6) passing the lithium-containing impurity-removing liquid into a bipolar membrane system to obtain a lithium hydroxide solution;
[0113] (7) Concentrating the lithium hydroxide solution by reverse osmosis to obtain a lithium-containing concentrated solution; and then evaporating and crystallizing the lithium-containing concentrated solution to obtain lithium hydroxide.
[0114] Example 2
[0115] The experimental steps and raw material ratios are the same as those in Example 1, except that the alkali material added in step (2) is a mixed alkali material, including calcium oxide, calcium hydroxide, magnesium hydroxide and magnesium oxide, wherein the mass ratio of each substance in the mixed alkali material is 45:15:30:10.
[0116] Example 3
[0117] The experimental steps and raw material ratios are the same as those in Example 1, except that the alkali material added in step (2) is a mixed alkali material, including calcium oxide, calcium hydroxide, sodium hydroxide, magnesium hydroxide and magnesium oxide, wherein the mass ratio of each substance in the mixed alkali material is 35:15:5:30:15.
[0118] Example 4
[0119] The experimental steps and raw material ratios are the same as those in Example 1, except that the alkali material added in step (2) is a mixed alkali material, including calcium oxide, calcium hydroxide, potassium hydroxide, magnesium hydroxide and magnesium oxide, wherein the mass ratio of each substance in the mixed alkali material is 35:15:5:30:15.
[0120] Example 5
[0121] The experimental steps and raw material ratios are the same as those in Example 1, except that in step (2), black powder and calcium oxide are mixed in a mass ratio of 1:0.5.
[0122] Example 6
[0123] The experimental steps and raw material ratios are the same as those in Example 1, except that in step (2), black powder and calcium oxide are mixed in a mass ratio of 1:0.8.
[0124] Example 7
[0125] The experimental steps and raw material ratios are the same as those in Example 1, except that in step (2), black powder and calcium oxide are mixed in a mass ratio of 1:2.
[0126] Example 8
[0127] The experimental steps and raw material ratios are the same as those in Example 1, except that in step (2), black powder and calcium oxide are mixed in a mass ratio of 1:3.
[0128] Example 9
[0129] The experimental steps and raw material ratios are the same as those of Example 2, except that after the roasted raw meal is obtained in step (2), the roasted raw meal is pressed into spherical raw meal with a particle size of 6 mm, and then the spherical raw meal is subjected to the roasting step of step (3).
[0130] Example 10
[0131] The experimental steps and raw material ratios are the same as those in Example 2, except that the calcination temperature in the tube furnace in step (3) is 1000°C.
[0132] Embodiment 11
[0133] The experimental steps and raw material ratios are the same as those in Example 2, except that the calcination temperature in the tube furnace in step (3) is 900°C.
[0134] Example 12
[0135] The experimental steps and raw material ratios are the same as those in Example 2, except that in step (4), the roasted clinker and the leaching agent are mixed at a solid-liquid mass ratio of 1:10.
[0136] Example 13
[0137] The experimental steps and raw material ratios are the same as those in Example 2, except that the leaching temperature in step (4) is 100°C.
[0138] Embodiment 14
[0139] The experimental steps and raw material ratios are the same as those in Example 2, except that the leaching time in step (4) is 3 h.
[0140] Comparative Example 1
[0141] The experimental steps and raw material ratios are the same as those in Example 1, except that calcium oxide is not added in step (2).
[0142] The lithium leaching rate, lithium recovery rate, impurity removal rate and lithium salt purity of the above Examples 1 to 14 and Comparative Example 1 were measured, and the test results are shown in Table 1 below:
[0143] Table 1:
[0144]
[0145]
[0146] Comparing the results of Example 1 and Comparative Example 1 in Table 1, it can be seen that the addition of alkali material can improve the purity of the product and the recovery rate and leaching rate of lithium. Comparing Example 1 with Example 2-4, it can be seen that the mixed alkali material is more conducive to the recovery of lithium in waste battery materials. Comparing Example 1 and Example 5-7, it can be seen that the optimal mass ratio of black powder to alkali material is 1:1. Comparing Example 2 and Example 9, it can be seen that making the roasted raw material into balls is beneficial to increase the contact area of the roasted raw material, improve the reaction efficiency, and increase the leaching rate and recovery rate of lithium. Comparing Examples 1, 10 and 11, it can be seen that if the roasting temperature is too high, the impurity metal in the black powder will melt, affecting the leaching of lithium. Comparing Examples 2 and 12-14, it can be seen that the change in the conditions of the leaching treatment has little effect on the leaching rate and recovery rate of lithium. This embodiment realizes the leaching of metallic lithium and the efficient preparation of battery-grade lithium hydroxide.
Claims
1. A method for recovering lithium from waste lithium-ion batteries, characterized in that: The method includes: Obtain black powder from used lithium-ion batteries; The black powder is mixed with an alkali material to obtain a roasted raw meal; Roasting the roasted raw material under aerobic conditions to obtain roasted clinker; The roasted clinker is mixed with a leaching agent for leaching to obtain a lithium-containing leaching solution; The lithium-containing leaching solution is crystallized to obtain lithium salt.
2. The method according to claim 1, wherein the mass ratio of the black powder to the alkali material is 1:(0.5-3); And / or, the alkali material comprises: At least one of sodium hydroxide, potassium hydroxide, calcium oxide, calcium hydroxide, magnesium hydroxide and magnesium oxide; And / or, the particle size of the black powder is 100-200 meshes.
3. The method according to claim 1, characterized in that The step of roasting the raw material under aerobic conditions to obtain roasted clinker comprises: Pressing the roasted raw material into spherical raw material with a particle size of 4 to 20 mm; The spherical raw material is roasted under aerobic conditions to obtain the roasted clinker.
4. The method according to claim 1, characterized in that The calcination temperature is 500-1000° C., and the calcination time is 0.5-12 hours.
5. The method according to claim 1, characterized in that The leaching temperature of the leaching treatment is 60-100°C, and the leaching time is 1-5h; And / or, the solid-to-liquid ratio between the roasted clinker and the leaching agent is 1:(3-30).
6. The method according to claim 1, characterized in that The step of subjecting the lithium-containing leachate to crystallization to obtain lithium salt comprises: The lithium-containing leaching solution is sequentially passed through a hydrogen-type cation exchange resin and a strong alkaline ion exchange resin to remove impurities, thereby obtaining a lithium-containing impurity-removed solution; The lithium-containing impurity-removing liquid is subjected to crystallization treatment to obtain the lithium salt.
7. The method according to claim 1, characterized in that The step of subjecting the lithium-containing leachate to crystallization to obtain lithium salt comprises: Passing the lithium-containing leaching solution into a bipolar membrane system to obtain a lithium hydroxide solution; The lithium hydroxide solution is subjected to crystallization treatment to obtain lithium hydroxide.
8. The method according to claim 7, characterized in that The acid solution produced by the bipolar membrane system is used to prepare the leaching agent.
9. The method according to claim 1, characterized in that The step of subjecting the lithium-containing leachate to crystallization to obtain lithium salt comprises: The lithium-containing leachate is subjected to reverse osmosis concentration to obtain a lithium-containing concentrated solution and a permeate; The lithium-containing concentrated solution is evaporated and crystallized to obtain the lithium salt and condensed water, wherein the condensed water and the permeate are used to prepare the leaching agent.
10. The method according to claim 1, characterized in that The step of mixing the black powder with an alkali material to obtain a roasted raw material comprises: The black powder and the alkali material are mixed and ground for 0.5 to 3 hours to obtain the roasted raw material.