System for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash

By overhauling the slag carbon slag aluminum ash preparation aluminum fluoride co-production lithium carbonate system, the problem of electrolytic aluminum hazardous waste disposal is solved, harmlessness and resource utilization are achieved, the yield of lithium ions is improved, and the environment and resource.

CN118754180APending Publication Date: 2024-10-11PUYANG RUIYUAN ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410855431.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

If hazardous solid waste such as overhaul slag, aluminum ash and carbon slag generated during the production of electrolytic aluminum is not properly disposed of, it will cause environmental harm and waste of resources. There is a lack of effective harmless and resource-based treatment technology.

Method used

A system for co-producing aluminum fluoride and lithium carbonate using overhaul slag, carbon slag, and aluminum ash. Through steps such as crushing, flotation, and hydrochloric acid solution treatment, the valuable components in the overhaul slag, carbon slag, and aluminum ash are separated and transformed to generate lithium carbonate and Aluminum fluoride.

Benefits of technology

It achieves comprehensive treatment of electrolytic aluminum solid hazardous waste, achieves harmlessness and resource utilization, increases the yield of lithium ions, and protects the environment and resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754180A_ABST
    Figure CN118754180A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic aluminum hazardous waste treatment, in particular to a system for preparing aluminum fluoride and co-producing lithium carbonate through overhaul slag, carbon slag and aluminum ash. Crushing the overhaul slag, the carbon slag and the aluminum ash respectively to obtain overhaul slag powder, carbon slag powder and aluminum ash powder for later use; the overhaul slag powder is leached with hydrochloric acid, and a leaching solution is obtained; performing flotation on the carbon residue powder through a flotation machine to obtain electrolyte powder; mixing the leachate, electrolyte powder and aluminum ash powder, and leaching with hydrochloric acid to obtain a liquid component and a solid component; taking the liquid component and adding sodium carbonate to obtain lithium carbonate; and mixing the solid component with the aluminum ash powder, and adding hydrochloric acid to obtain the aluminum fluoride. According to the method, comprehensive treatment of the electrolytic aluminum solid hazardous waste can be achieved, lithium carbonate and aluminum fluoride are prepared, harmlessness and recycling of the electrolytic aluminum solid hazardous waste are achieved, and resource saving and environment protection are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hazardous waste treatment of electrolytic aluminum, and in particular to a system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash. Background Art

[0002] Electrolytic aluminum is the process of extracting metallic aluminum from alumina through electrolysis. Metallic aluminum is relatively active and exists in the form of metal oxides in nature. It is difficult to prepare metallic aluminum using traditional methods. In industrial production, it can only be prepared through electrolysis. Since metallic aluminum products are widely used, the electrolytic aluminum industry plays a significant role in the process of social development.

[0003] However, a large amount of hazardous waste is generated in the process of preparing metallic aluminum through electrolysis, such as overhaul slag, aluminum ash, carbon slag, etc.; among them, overhaul slag is the waste slag generated by repairing and replacing the cathode lining of the electrolytic cell in the production of electrolytic aluminum. It is mainly composed of waste cathode carbon blocks, waste refractory materials, waste cathode steel bars and cathode ash, and contains a large amount of soluble fluoride. If it is not properly disposed of, it will cause great environmental harm and safety hazards; aluminum ash is the aluminum ash slag generated on the surface of the melt during the processes of aluminum liquid transfer, refining, alloying, casting, etc. in the production of electrolytic aluminum, as well as salt slag and secondary aluminum ash slag generated in the aluminum recovery process, which contains a large amount of soluble fluoride. Ammonia and methane will be generated when aluminum nitride and aluminum carbide in aluminum ash react with water, which will cause harm to humans and threaten the ecological environment; carbon slag is mainly waste generated by the shedding of carbon particles caused by uneven combustion and selective oxidation of carbon anodes, or the shedding of carbon particles of carbon cathodes under the erosion and scouring of aluminum liquid and electrolytes. In addition to 20-30% carbon, it also contains 60-70% electrolyte, among which the main components of the electrolyte are Na3AlF6, AlF3 and LiF, which are also very harmful to the environment and human body.

[0004] According to statistics, every ton of electrolytic aluminum produced will produce 15-20kg of overhaul slag, 6.3-10kg of aluminum ash, and 10-12kg of carbon slag. The total amount of typical hazardous solid wastes such as overhaul slag, aluminum ash and carbon slag generated by my country's electrolytic aluminum enterprises each year exceeds 1.2 million tons. If not properly disposed of, it will cause great environmental damage and safety hazards, and will also cause the loss of resources. Therefore, a treatment system that can dispose of electrolytic aluminum hazardous waste to achieve harmlessness and resource utilization of electrolytic aluminum hazardous waste is an urgent problem to be solved. Summary of the invention

[0005] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and provide a system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash, so as to achieve comprehensive treatment of hazardous waste from electrolytic aluminum, thereby realizing the purpose of harmless treatment and resource utilization of hazardous waste from electrolytic aluminum.

[0006] To achieve the above object, the present invention adopts the following technical scheme: a system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash, characterized in that it comprises the following steps:

[0007] S1. Crush the overhaul slag, carbon slag and aluminum ash respectively to obtain overhaul slag powder, carbon slag powder and aluminum ash powder respectively, and then set aside;

[0008] S2. Leach the overhaul slag powder with a hydrochloric acid solution to obtain a leachate; flotate the carbon slag powder with a flotation machine to obtain an electrolyte powder;

[0009] S3, mixing the leaching solution, the electrolyte powder and the aluminum ash powder, and leaching with a hydrochloric acid solution to obtain a liquid component and a solid component;

[0010] S4, taking the liquid component and adding sodium carbonate solution to obtain lithium carbonate;

[0011] S5. Mix the solid component with aluminum ash powder and add hydrochloric acid solution to obtain aluminum fluoride.

[0012] Furthermore, in the above S1, the overhaul slag, carbon slag and aluminum ash are crushed to a size of 200-300 meshes.

[0013] Furthermore, in the S2, the mass fraction of the hydrochloric acid solution is 20%, and the mass ratio of the overhaul slag powder to the hydrochloric acid solution is 1 to 1.5:1.

[0014] Furthermore, in the S3, the mass ratio of the leaching solution, the electrolyte powder, the aluminum ash powder and the hydrochloric acid solution is 1:0.5-2:0.5-1:2-3.

[0015] Furthermore, the liquid component is a lithium-rich solution, and the solid component is a mixture of Na3AlF6 and aluminum fluoride.

[0016] Furthermore, in the S4, the mass ratio of the liquid component to the sodium carbonate in the sodium carbonate solution is 3 to 5:1.

[0017] Furthermore, in the S5, the mass ratio of the solid component, the aluminum ash powder and the hydrochloric acid solution is 1:0.2-0.5:2-5.

[0018] Beneficial effects of the present invention:

[0019] 1. It can realize the comprehensive treatment of solid hazardous waste from electrolytic aluminum, realize the harmlessness and resource utilization of solid hazardous waste from electrolytic aluminum, and is conducive to resource conservation and environmental protection;

[0020] 2. The method of dissolving lithium first and then sodium is helpful for the precipitation of lithium ions and the improvement of the yield of lithium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the system flow of the present invention. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0023] like Figure 1 As shown, in the processing system of this embodiment, the carbon slag is crushed by ball mill A to obtain carbon slag powder, and the carbon slag powder is floated by a flotation machine to obtain carbon powder and electrolyte powder, and the electrolyte powder is transported to reaction tank A.

[0024] The overhaul slag is crushed by ball mill B to obtain overhaul slag powder, which is added to reaction tank B. Reaction tank B is connected to nitric acid storage tank, which transports nitric acid to reaction tank B. After the overhaul slag powder reacts with nitric acid in reaction tank B, solid-liquid separation is performed, the solid phase is mainly refractory material, and the liquid phase is passed into reaction tank A.

[0025] The above-mentioned electrolyte powder and the liquid phase after solid-liquid separation of reaction tank B are both introduced into reaction tank A, which is connected to a hydrochloric acid storage tank, which introduces hydrochloric acid into reaction tank A, and adds aluminum ash powder into reaction tank A; the hydrochloric acid, aluminum ash powder and electrolyte powder react and then undergo solid-liquid separation to obtain a solid component and a liquid component; the liquid component is introduced into reaction tank C, which is connected to a sodium carbonate storage tank, and sodium carbonate is added to reaction tank C through the sodium carbonate storage tank, and the sodium carbonate and the liquid component react to generate lithium carbonate, and lithium carbonate is obtained after solid-liquid separation of the reaction liquid.

[0026] The solid component obtained in the above reaction tank A is added to the reaction tank D, and the reaction tank D is connected to the hydrochloric acid storage tank, and hydrochloric acid is passed into the reaction tank D from the hydrochloric acid storage tank; the aluminum ash is crushed by the ball mill C to obtain aluminum ash powder, and the aluminum ash powder is added to the reaction tank D, and the aluminum ash powder, hydrochloric acid and solid components react in the reaction tank D, and aluminum fluoride is obtained after solid-liquid separation.

[0027] The principle of the present invention is:

[0028] The main components of overhaul slag are refractory materials and electrolytes, among which the electrolyte mainly contains Na3AlF6, Li3AlF6, etc. Under the condition of hydrochloric acid, Na3AlF6 and Li3AlF6 react with hydrochloric acid in reaction tank B. The reaction mechanism is as follows:

[0029] Li3AlF6+3HCl=3LiCl+3HF+AlF3↓

[0030] Na3AlF6+3HCl=3NaCl+3HF+AlF3↓

[0031] In this step, the amount of hydrochloric acid is controlled to be excessive, so that the fluorine and lithium in the overhaul slag can be dissolved, and the aluminum fluoride generated by the reaction is mixed with the refractory material that does not participate in the reaction and discharged from the reaction system through solid-liquid separation.

[0032] In actual production, the fluorine content in the overhaul slag is generally around 10%, and the concentration of commonly used hydrochloric acid is around 20%. The mass ratio of the overhaul slag to the hydrochloric acid solution is controlled at 1 to 1.5:1, which can well achieve the dissolution of fluorine in the overhaul slag (about 50% can be recovered, and the rest is formed into aluminum fluoride precipitate and mixed with refractory materials). During the process, the reaction temperature is controlled at 70 to 80°C, the reaction time is 2 to 4 hours, and the stirring intensity is 300r / min.

[0033] It should be noted that in this step, lithium ions will dissolve before sodium ions, but for overhaul slag, the purpose is to dissolve fluorine and lithium. Therefore, there is no need to subdivide in this step, and it is sufficient to control the excess of hydrochloric acid.

[0034] The main components of carbon slag are carbon powder and electrolyte. The carbon powder and electrolyte can be separated by a flotation machine. In the reaction tank A, some aluminum ash powder (mainly composed of aluminum oxide) is added, and the amount of hydrochloric acid added is controlled, that is, the mass ratio of the leaching solution, electrolyte powder, aluminum ash powder and hydrochloric acid solution is 1:0.5-2:0.5-1:2-3, so that the reaction stays at the lithium dissolving stage. The reaction mechanism is as follows:

[0035] Li3AlF6+3HCl=3LiCl+3HF+AlF3↓

[0036] Al2O3+6HF=3H2O+2AlF3↓

[0037] After the above reaction is completed, solid-liquid separation is performed to obtain a solid component and a liquid component, wherein the solid component contains Na3AlF6 and aluminum fluoride, and the liquid component is enriched with lithium chloride. The liquid component is passed into a reaction tank C, and a sodium carbonate solution is added to the reaction tank C. The mass ratio of sodium carbonate in the sodium carbonate solution is 3 to 5:1, so lithium carbonate can be obtained after solid-liquid separation. The mechanism is as follows:

[0038] 2LiCl+Na2CO3=2NaCl+Li2CO3↓

[0039] The solid component obtained by the above reaction is added to the reaction tank D, and hydrochloric acid is continuously added to the reaction tank D, so that the sodium ions can be dissolved, and aluminum ash powder is added to precipitate and neutralize the hydrofluoric acid generated by the reaction. The mass ratio of the solid component, aluminum ash powder and hydrochloric acid solution is 1:0.2-0.5:2-5. Aluminum fluoride can be obtained after solid-liquid separation. The mechanism is as follows:

[0040] Na3AlF6+3HCl=3NaCl+3HF+AlF3↓

[0041] Al2O3+6HF=3H2O+2AlF3↓

[0042] AlCl3+3HF=3HCl+AlF3↓

[0043] Al2O3+6HCl=2AlCl3+3H2O

[0044] Therefore, through the treatment system of the present invention, it is possible to treat solid hazardous wastes such as overhaul slag, carbon slag and aluminum ash produced by electrolytic aluminum, and obtain lithium carbonate and aluminum fluoride, thereby achieving the harmlessness and resource utilization of solid hazardous wastes of electrolytic aluminum, which is beneficial to resource conservation and environmental protection.

Claims

1. A system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash, characterized in that: The following steps are involved: S1. Crush the overhaul slag, carbon slag and aluminum ash respectively to obtain overhaul slag powder, carbon slag powder and aluminum ash powder respectively, and then set aside; S2. Leach the overhaul slag powder with a hydrochloric acid solution to obtain a leachate; flotate the carbon slag powder with a flotation machine to obtain an electrolyte powder; S3, mixing the leaching solution, the electrolyte powder and the aluminum ash powder, and leaching with a hydrochloric acid solution to obtain a liquid component and a solid component; S4, taking the liquid component and adding sodium carbonate solution to obtain lithium carbonate; S5. Mix the solid component with aluminum ash powder and add hydrochloric acid solution to obtain aluminum fluoride.

2. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 1, characterized in that: In the above-mentioned S1, the overhaul slag, carbon slag and aluminum ash are crushed to a size of 200-300 meshes.

3. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 1, characterized in that: In the S2, the mass fraction of the hydrochloric acid solution is 20%, and the mass ratio of the overhaul slag powder to the hydrochloric acid solution is 1-1.5:

1.

4. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 3, characterized in that: In the S3, the mass ratio of the leaching solution, the electrolyte powder, the aluminum ash powder and the hydrochloric acid solution is 1:0.5-2:0.5-1:2-3.

5. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 4, characterized in that: The liquid component is a lithium-rich solution, and the solid component is a mixture of Na3AlF6 and aluminum fluoride.

6. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 1, characterized in that: In the S4, the mass ratio of the liquid component to the sodium carbonate in the sodium carbonate solution is 3 to 5:

1.

7. The system for preparing aluminum fluoride and co-producing lithium carbonate from overhaul slag, carbon slag and aluminum ash according to claim 3, characterized in that: In the S5, the mass ratio of the solid component, the aluminum ash powder and the hydrochloric acid solution is 1:0.2-0.5:2-5.

Citation Information

Cited By

  • Method for extracting lithium from surface shell material and overhaul slag and co-producing steel mill slagging agent