Method for improving chromium-doped crystallization rate of ammonium paratungstate
By adding chromium acetate and a crystallization promoter into the ammonium tungstate solution, the problem of uneven doping in tungsten powder is solved, the crystallization rate of chromium and the properties of cemented carbide are improved, and the difficulty of chromium recycling and environmental protection are reduced. Processing costs.
Patent Information
- Application Number
- CN202410889299.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing technology, tungsten powder doped with carbide powder is difficult to mix evenly, causing the tungsten carbide grains to grow unexpectedly and affecting the performance of the cemented carbide. Moreover, the crystallization rate of chromium doped in ammonium paratungstate is low, which increases the difficulty of recycling chromium. and environmental disposal requirements.
By adding chromium acetate to the ammonium tungstate solution and then stirring and evaporating for crystallization, adding a crystallization promoter when the appropriate pH value is detected, continuing stirring, evaporating, crystallizing and filtering, the crystallization rate of chromium-doped ammonium paratungstate can be increased.
The crystallization rate of chromium is increased from 50 to 55% to 70 to 80%, ensuring the uniformity and environmental friendliness of chromium, reducing the chromium content rate in the solution, and enhancing the chromium doping effect.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tungsten smelting and processing, and particularly relates to a method for improving the crystallization rate of ammonium paratungstate doped with chromium. Background Art
[0002] Ultrafine cemented carbide doped with grain growth inhibitors is widely used in modern tool materials, wear-resistant materials, high temperature resistant and corrosion-resistant materials due to its high melting point, high hardness and high strength. There are many types of grains that control the growth of tungsten carbide grains. Currently, vanadium carbide or chromium carbide is widely used in production to control the growth of tungsten carbide matrix during sintering. At present, doping mainly adopts the solid-solid doping process before tungsten powder carburization, and the inhibitor carbide powder is added to the tungsten powder in the form of inhibitor carbide powder. However, the inhibitors of the above method are difficult to mix evenly, resulting in the unexpected growth of some tungsten carbide grains during the sintering process of tungsten carbide, which in turn affects the performance of cemented carbide. Some researchers have also proposed a method of doping chromium in ammonium paratungstate, that is, adding chromium acetate and other substances to evaporate and crystallize together during the evaporation and crystallization process to achieve a uniform mixing effect. However, the crystallization rate of chromium is only about 50-55%, which inevitably increases the difficulty of chromium recycling. In addition, chromium is a toxic metal, and the undoped chromium can only be left in the solution for wastewater treatment, which inevitably increases the industrial technical requirements and economic requirements for environmental protection treatment. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for improving the crystallization rate of ammonium paratungstate doped with chromium.
[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0005] A method for improving the crystallization rate of ammonium paratungstate doped with chromium comprises the following steps:
[0006] S1, take ammonium tungstate solution, add chromium acetate to dissolve it, and then stir and evaporate to crystallize;
[0007] S2. When the pH value of the detection solution is 7-7.3, a crystallization promoting agent is added to the solution, and the solution is continuously stirred for evaporation and crystallization, and then filtered to improve the crystallization rate of ammonium paratungstate doped with chromium.
[0008] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S1, the concentration of the ammonium tungstate solution is 200-250 g / L in terms of tungsten trioxide.
[0009] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S1, the temperature of evaporation and crystallization is 90-120°C.
[0010] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S1, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200-350 r / min.
[0011] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S1, the solid-liquid ratio of the added amount of chromium acetate to the ammonium tungstate solution is 1g:(25-100)mL.
[0012] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, the crystallization promoting agent is ammonium sulfate or ammonium sulfite.
[0013] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, the amount of the crystallization promoter added is 50-80wt% of the mass of chromium acetate.
[0014] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, a crystallization promoting agent is added, and the mixture is stirred for evaporation and crystallization, and filtered when the pH value is 6.4 to 6.7.
[0015] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, the temperature of evaporation and crystallization is 90-120°C.
[0016] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200-350 r / min.
[0017] As a preferred embodiment of the method for improving the crystallization rate of chromium-doped ammonium paratungstate described in the present invention, wherein: in the step S2, the chromium ions in the solution are detected after filtration, and the crystallization rate of the chromium ions is 70-80%.
[0018] The beneficial effects of the present invention are as follows:
[0019] The present invention provides a method for improving the crystallization rate of ammonium paratungstate doped with chromium, by reasonably regulating the evaporation crystallization temperature curve of chromium, and adding a crystallization promoter for improving the crystallization rate of chromium to the solution at a suitable time during the evaporation crystallization process. The present invention does not add new impurities, and can improve the crystallization rate of chromium and reduce the chromium content in the solution on the basis of ensuring the uniformity of chromium, thereby ensuring environmental friendliness and improving the chromium doping effect. DETAILED DESCRIPTION
[0020] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] According to one aspect of the present invention, the present invention provides the following technical solution:
[0022] A method for improving the crystallization rate of ammonium paratungstate doped with chromium comprises the following steps:
[0023] S1, take ammonium tungstate solution, add chromium acetate to dissolve it, and then stir and evaporate to crystallize;
[0024] S2. When the pH value of the detection solution is 7-7.3, a crystallization promoting agent is added to the solution, and the solution is continuously stirred for evaporation and crystallization, and then filtered to improve the crystallization rate of ammonium paratungstate doped with chromium.
[0025] The invention adds a crystallization promoting agent for increasing the chromium crystallization rate to the solution at an appropriate time during the evaporation crystallization process. The invention does not add new impurities, and can increase the chromium crystallization rate and reduce the chromium content in the solution on the basis of ensuring the uniformity of chromium.
[0026] Preferably, in step S1, the concentration of the ammonium tungstate solution is 200-250 g / L in terms of tungsten trioxide.
[0027] Preferably, in step S1, the temperature of evaporation crystallization is 90-120°C.
[0028] Preferably, in step S1, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200 to 350 r / min.
[0029] Preferably, in step S1, the solid-liquid ratio of the added amount of chromium acetate to the ammonium tungstate solution is 1 g: (25-100) mL.
[0030] Preferably, in step S2, the crystallization agent is ammonium sulfate or ammonium sulfite.
[0031] Preferably, in step S2, the amount of the crystallization agent added is 50-80wt% of the mass of chromium acetate.
[0032] Preferably, in step S2, a crystallization promoting agent is added, the mixture is stirred for evaporation and crystallization, and the mixture is filtered when the pH value is 6.4 to 6.7.
[0033] Preferably, in step S2, the temperature of evaporation crystallization is 90-120°C.
[0034] Preferably, in step S2, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200 to 350 r / min.
[0035] Preferably, in step S2, the chromium ions in the solution are detected after filtration, and the chromium ion crystallization rate is 70-80%, which is increased from 50-55% in the prior art to 70-80%.
[0036] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0037] Example 1
[0038] A method for improving the crystallization rate of ammonium paratungstate doped with chromium comprises the following steps:
[0039] S1. Take 500 mL of ammonium tungstate solution, add 10 g of chromium acetate to dissolve it, and then stir to evaporate and crystallize; the concentration of the ammonium tungstate solution is 250 g / L in terms of tungsten trioxide; the temperature of evaporation and crystallization is 100°C; the stirring adopts a positive and negative alternating stirring method, and the stirring speed is 200 r / min;
[0040] S2. When the pH of the test solution is 7, add a crystallization agent to the solution, continue stirring to evaporate and crystallize, and then filter to improve the crystallization rate of ammonium paratungstate doped with chromium. The crystallization agent is ammonium sulfate, the amount of the crystallization agent added is 5g, the temperature of evaporation and crystallization is 100℃; the stirring adopts the positive and negative alternating stirring method, and the stirring speed is 200r / min; add the crystallization agent, stir and evaporate and crystallize, filter when the pH is 6.5, and detect the chromium ions in the solution after filtration. The chromium ion crystallization rate is 76%.
[0041] Example 2
[0042] A method for improving the crystallization rate of ammonium paratungstate doped with chromium comprises the following steps:
[0043] S1. Take 500 mL of ammonium tungstate solution, add 5 g of chromium acetate to dissolve it, and then stir to evaporate and crystallize; the concentration of the ammonium tungstate solution is 200 g / L in terms of tungsten trioxide; the temperature of evaporation and crystallization is 120°C; the stirring adopts a positive and negative alternating stirring method, and the stirring speed is 200 r / min;
[0044] S2. When the pH of the test solution is 7.3, add a crystallization agent to the solution, continue stirring to evaporate and crystallize, and then filter to improve the crystallization rate of ammonium paratungstate doped with chromium. The crystallization agent is ammonium sulfite, the amount of the crystallization agent added is 4g, the temperature of evaporation and crystallization is 120℃; the stirring adopts the method of alternating positive and negative stirring, and the stirring speed is 200r / min; add the crystallization agent, stir and evaporate and crystallize, filter when the pH is 6.7, and detect the chromium ions in the solution after filtration. The chromium ion crystallization rate is 73%.
[0045] Example 3
[0046] A method for improving the crystallization rate of ammonium paratungstate doped with chromium comprises the following steps:
[0047] S1. Take 500 mL of ammonium tungstate solution, add 20 g of chromium acetate to dissolve it, and then stir to evaporate and crystallize; the concentration of the ammonium tungstate solution is 250 g / L in terms of tungsten trioxide; the temperature of evaporation and crystallization is 120°C; the stirring is carried out by alternating forward and reverse stirring at a stirring speed of 350 r / min;
[0048] S2. When the pH of the test solution is 7.3, add a crystallization agent to the solution, continue stirring to evaporate and crystallize, and then filter to improve the crystallization rate of ammonium paratungstate doped with chromium. The crystallization agent is ammonium sulfate, the amount of the crystallization agent added is 12g, the temperature of evaporation and crystallization is 120℃; the stirring adopts the method of alternating positive and negative stirring, and the stirring speed is 200r / min; add the crystallization agent, stir and evaporate and crystallize, filter when the pH is 6.4, and detect the chromium ions in the solution after filtration. The chromium ion crystallization rate is 78%.
[0049] Comparative Example 1
[0050] The difference from Example 3 is that no crystallization agent is added in step S2.
[0051] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 65%.
[0052] Comparative Example 2
[0053] The difference from Example 3 is that the stirring in steps S1 and S2 is carried out in one direction.
[0054] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 66%.
[0055] Comparative Example 3
[0056] The difference from Example 3 is that the stirring speed in steps S1 and S2 is 180 r / min.
[0057] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 68%.
[0058] Comparative Example 4
[0059] The difference from Example 3 is that the temperature of evaporation crystallization in steps S1 and S2 is 80°C.
[0060] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 67%.
[0061] Comparative Example 5
[0062] The difference from Example 3 is that the stirring in steps S1 and S2 is carried out in one direction, and no crystallization agent is added in step S2.
[0063] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 52%.
[0064] Comparative Example 6
[0065] The difference from Example 3 is that when the pH of the test solution is 8, a crystallization promoting agent is added to the solution.
[0066] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 65%.
[0067] Comparative Example 7
[0068] The difference from Example 3 is that ammonium chloride is used instead of ammonium sulfate.
[0069] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 62%.
[0070] Comparative Example 8
[0071] The difference from Example 3 is that the amount of the crystallization agent added is 4 g.
[0072] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 63%.
[0073] Comparative Example 9
[0074] The difference from Example 3 is that the amount of the crystallization agent added is 10 g.
[0075] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 66%.
[0076] Comparative Example 10
[0077] The difference from Example 3 is that the added amount of chromium acetate is 3 g.
[0078] After filtering, the chromium ions in the solution were detected, and the chromium ion crystallization rate was 48%.
[0079] It can be seen from the above embodiments and comparative examples that the present invention reasonably regulates the evaporation and crystallization temperature curve of chromium and adds a crystallization promoter for increasing the chromium crystallization rate to the solution at an appropriate time during the evaporation and crystallization process. The present invention does not add new impurities, and can increase the chromium crystallization rate and reduce the chromium content in the solution on the basis of ensuring the uniformity of chromium, thereby ensuring environmental friendliness and improving the chromium doping effect.
[0080] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for improving the crystallization rate of ammonium paratungstate doped with chromium, characterized in that: The steps include: S1, take ammonium tungstate solution, add chromium acetate to dissolve it, and then stir and evaporate to crystallize; S2. When the pH value of the detection solution is 7-7.3, a crystallization promoting agent is added to the solution, and the solution is continuously stirred for evaporation and crystallization, and then filtered to improve the crystallization rate of ammonium paratungstate doped with chromium.
2. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S1, the concentration of the ammonium tungstate solution is 200-250 g / L in terms of tungsten trioxide.
3. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S1, the temperature of evaporation crystallization is 90-120°C.
4. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S1, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200-350 r / min.
5. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S1, the solid-liquid ratio of the added amount of chromium acetate to the ammonium tungstate solution is 1 g: (25-100) mL.
6. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S2, the crystallization agent is ammonium sulfate or ammonium sulfite, and the amount of the crystallization agent added is 50-80wt% of the mass of chromium acetate.
7. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S2, a crystallization promoting agent is added, and the mixture is stirred for evaporation and crystallization, and filtered when the pH value is 6.4 to 6.
7.
8. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S2, the temperature of evaporation crystallization is 90-120°C.
9. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In step S2, the stirring is carried out in a forward and reverse alternating stirring manner, and the stirring speed is 200-350 r / min.
10. The method for improving the crystallization rate of ammonium paratungstate doped with chromium according to claim 1, characterized in that: In the step S2, the chromium ions in the solution are detected after filtering, and the chromium ion crystallization rate is 70-80%.