By combining the in-situ method and the surface modification method, a high-temperature-resistant wave-transmitting heat-insulating airgel material is prepared, which solves the problem in the existing technology that airgel materials are difficult to reuse in high-temperature environments, and achieves high temperature resistance at 500°C. Excellent hydrophobic and thermal insulation properties.
Patent Information
- Application Number
- CN202410960906.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Existing airgel wave-transmitting thermal insulation materials are difficult to reuse in high-temperature environments, and their hydrophobic effects are reduced or invalidated, resulting in a decline in wave-transmitting thermal insulation performance.
Using a preparation method that combines in-situ method and surface modification method, silicon source, hydrophobic agent, alcohol substances, acid catalyst and alkali catalyst are used to configure the sol, and through supercritical drying and post-heat treatment, high temperature resistant nano-inorganic oxides and Surface modifier to prepare wave-transmitting and heat-insulating aerogel materials with super-hydrophobic properties and high temperature resistance.
The prepared wave-transmitting heat-insulating aerogel material still maintains good hydrophobic effect and wave-transmitting heat-insulating properties after 10 times of heat treatment at 500°C and 2 hours. It has low mass loss rate, large contact angle, and dielectric constant and dielectric properties after moisture absorption. The electrical loss angle is within a reasonable range, and the thermal conductivity at room temperature is appropriate.
Smart Images

Figure CN118754597A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerogel materials, and in particular relates to a reusable wave-transmitting heat-insulating aerogel material and a preparation method thereof. Background Art
[0002] Wave-transmitting heat-insulating aerogel materials are widely used in aerospace, weapons and equipment, etc., due to their high efficiency in heat insulation and high wave transmission. The development of reusable space shuttles is an important development direction in the aerospace field, so the reusability of aerogel materials is required.
[0003] Existing aerogel wave-transmitting and heat-insulating composite materials usually replace their surface hydrophilic groups through hydrophobic modification to maintain their excellent properties of high efficiency heat insulation and high wave transmission. There are two commonly used methods for hydrophobic modification of aerogel materials: one is the in-situ polymerization method, that is, adding silicon alkoxide containing hydrophobic groups to the sol-gel system, compounding the sol with fibers, and obtaining a hydrophobic aerogel wave-transmitting and heat-insulating composite material through gelation, aging, and supercritical drying processes; the other is the surface post-treatment method, also called surface modification method, which is a commonly used surface modification process. The key is to inertize and replace the -OH groups with strong surface polarity, thereby forming non-polar or weakly polar -OR (R is any aliphatic group), so that the hydrophilic aerogel is transformed into a hydrophobic aerogel. However, most hydrophobic modifications use low surface energy organic hydrophobic agents, which can generally withstand temperatures below 400°C. When working in a high temperature environment for a long time, the organic matter will gradually decompose, reducing or making the hydrophobic effect ineffective. When absorbing moisture or encountering water, the structure will collapse and powderize, resulting in a serious decline or even loss of wave-transmitting and heat-insulating performance.
[0004] Therefore, reusable wave-transmitting and heat-insulating aerogel materials have become an urgent need in the aerospace field. Summary of the invention
[0005] In view of the problem that aerogel wave-transmitting and heat-insulating materials in the prior art are difficult to reuse, the present invention provides a reusable hydrophobic aerogel wave-transmitting and heat-insulating material and a preparation method thereof. The wave-transmitting and heat-insulating aerogel material prepared by the method can still maintain good wave-transmitting and heat-insulating properties after 10 heat treatments at 500°C and 2h.
[0006] The purpose of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a reusable wave-transmitting heat-insulating aerogel material comprises the following steps:
[0008] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1: (0.25-1): (3-4): (5-20): 1.8×10 -3 :3.6×10-2 Prepare sol;
[0009] The silicon source is selected from one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate and isopropyl orthosilicate;
[0010] The hydrophobic agent is selected from one of phenyltrimethoxysilane (PTMS), phenyltriethoxysilane (PTES), and methyltriethoxysilane (MTEOS);
[0011] The alcohol substance is selected from one of methanol, ethanol, isopropanol, n-butanol, sec-butanol and tert-butanol;
[0012] The acid catalyst is selected from hydrochloric acid, nitric acid and sulfuric acid;
[0013] The alkaline catalyst is selected from aqueous ammonia;
[0014] Sol preparation is carried out in two steps:
[0015] A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 of the mass of the alcohol substance, 1 / 2 of the mass of the deionized water and the acid catalyst, mix and stir evenly to obtain solution ①, add the silicon source dropwise to solution ①, stir and hydrolyze at 40℃-50℃ for 2h-4h to obtain solution ②;
[0016] B. According to the molar ratio of the sol, 1 / 3 of the alcohol substance, the remaining deionized water and the alkaline catalyst are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0017] 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain a concentration of 0.003-0.006 mol / L Ce(NO 3 ) 3 The solution was finally stirred for 5 h in a water bath at 30 °C to obtain a modifier;
[0018] 3) Preform molding: Preform the inorganic fiber at 0.1-0.25g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0019] The inorganic fiber is selected from one of glass fiber, basalt fiber and quartz fiber;
[0020] 4) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; 2After the nanoparticle sol and the modifier obtained in step 2) are uniformly mixed, they are slowly pumped into the glue box under the conditions of -0.06 to -0.1 MPa and -5 to 0°C. When the sol liquid surface immerses the preform, the pressure is maintained in a vacuum impregnation tank for 1 to 4 hours to fully impregnate it;
[0021] 5) Gel and aging treatment: seal the glue box after impregnation and place it in a 40°C environment to wait for gelation. After gelation, add alcohol substances to the glue box to protect the gel surface from cracking. After sealing, keep it in a 40°C environment for aging for 12-48 hours;
[0022] The alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0023] 6) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 260-280°C, the pressure is 8-12MPa, and the drying time is 4-8h to obtain a modified aerogel thermal insulation composite material;
[0024] 7) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 260-300° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material;
[0025] 8) Surface modification: 1H,1H,2H,2H-perfluorodecyltriethoxysilane (PFDTES) was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L;
[0026] Then, the wave-transmitting heat-insulating aerogel material prepared in step 6) is placed in a container and placed in a vacuum impregnation tank. The surface modifier is slowly pumped into the container at 40°C and -0.1MPa vacuum to fully impregnate the wave-transmitting heat-insulating aerogel material, and the surface modifier is kept for 12 hours. After being taken out, the material is heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material. The reusable wave-transmitting heat-insulating aerogel material is placed in a muffle furnace at 500°C and 2h. After 10 times of medium heat treatment, it still has excellent hydrophobic effect and wave-transmitting heat-insulating performance, the mass loss rate is 1.56-3.85%, the contact angle is 140.6°-160.5°, the mass moisture absorption rate is 0.98-1.90%, and it still has excellent wave-transmitting heat-insulating performance. After moisture absorption, the dielectric constant is 1.3-2.1, the dielectric loss tangent is 0.004-0.009 (10GHz), and the thermal conductivity at room temperature is 0.020-0.030W / mK.
[0027] Furthermore, the strong stirring condition in step 2) has a rotation speed of 800-1000 rpm; the stirring condition has a rotation speed of 100-200 rpm; and the continuous stirring has a rotation speed of 100-200 rpm.
[0028] The present invention also relates to a reusable wave-transmitting heat-insulating aerogel material, which is obtained by the preparation method of the reusable wave-transmitting heat-insulating aerogel material. The reusable wave-transmitting heat-insulating aerogel material is placed in a muffle furnace at 500°C for 2h for heat treatment 10 times, and still has excellent hydrophobic effect and wave-transmitting heat-insulating performance, a mass loss rate of 1.56-3.85%, a contact angle of 140.6°-160.5°, a mass moisture absorption rate of 0.98-1.90%, and still has excellent wave-transmitting heat-insulating performance, a dielectric constant of 1.3-2.1 after moisture absorption, a dielectric loss tangent of 0.004-0.009 (10GHz), and a thermal conductivity of 0.020-0.030W / mK at room temperature.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] 1. The preparation method of a reusable wave-transmitting heat-insulating aerogel material described in the present invention adopts an in-situ method + surface modification method to prepare a wave-transmitting heat-insulating aerogel material with super-hydrophobic properties; the in-situ method has a simple and easy-to-control formula, and does not add complicated process steps. While making the aerogel material hydrophobic, it introduces high-temperature-resistant nano-inorganic oxide cerium oxide, and then grafts PFDTES through a surface modification method to further improve hydrophobicity and temperature resistance. The combination of the two methods makes the hydrophobic effect of the aerogel material controllable, the formula controllable, the hydrophobic uniformity is good, the material has super-hydrophobicity both inside and outside, and at the same time makes the aerogel temperature resistance better and has reusable performance.
[0031] 2. The reusable wave-transmitting and heat-insulating aerogel material described in the present invention is placed in a muffle furnace for heat treatment for 10 times at 500°C for 2 hours and still has excellent hydrophobic effect and wave-transmitting and heat-insulating performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a process flow chart of a method for preparing a reusable wave-transmitting heat-insulating aerogel material according to the present invention;
[0033] Figure 2 This is a picture of the hydrophobic surface of the reusable wave-transmitting heat-insulating aerogel material prepared in Example 3 of the present invention, which has been heat-treated 10 times in a muffle furnace at 500° C. for 2 h;
[0034] Figure 3 This is a surface image of the wave-transmitting and heat-insulating aerogel material prepared in Comparative Example 1 of the present invention, which is heat-treated 10 times in a muffle furnace at 500° C. for 2 hours. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below by way of examples, but these examples should not be considered as limiting the present invention.
[0036] In the embodiments and comparative examples:
[0037] The contact angle was measured by a video contact angle meter.
[0038] The mass moisture absorption data is measured in accordance with GB / T 5480-2008.
[0039] The dielectric constant and dielectric loss tangent are measured according to DqES423-2006.
[0040] The room temperature thermal conductivity data is measured according to GB / T10295-2008.
[0041] Embodiment 1:
[0042] A method for preparing a reusable wave-transmitting heat-insulating aerogel material comprises the following steps:
[0043] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst were mixed in a molar ratio of 1:0.75:3:5:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0044] The silicon source is methyl orthosilicate;
[0045] The hydrophobic agent is PTMS;
[0046] The alcohol substance is methanol;
[0047] The acid catalyst is hydrochloric acid;
[0048] The alkaline catalyst is selected from aqueous ammonia;
[0049] Sol preparation is carried out in two steps:
[0050] A. According to the molar ratio of the sol, take the whole mass of the hydrophobic agent, 2 / 3 mass of methanol, 1 / 2 mass of deionized water and hydrochloric acid, mix and stir evenly to obtain solution ①, add methyl orthosilicate dropwise to solution ①, stir and hydrolyze at 40°C for 2h to obtain solution ②;
[0051] B. According to the molar ratio of the sol, 1 / 3 of the mass of methanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0052] 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain a 0.003 mol / L concentration of Ce(NO 3 ) 3solution; finally, stirring was continued for 5 h in a water bath at 30°C to obtain a modifier;
[0053] 3) Preform molding: The inorganic fiber is pressed at 0.20g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0054] The inorganic fiber is selected from glass fiber;
[0055] 4) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box under -0.1MPa and 0°C. When the sol liquid level exceeds the upper edge of the preform by 5-10mm, maintain the pressure in the vacuum impregnation tank for 2h to fully impregnate it;
[0056] 5) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 12 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0057] 6) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 260°C, the pressure is 8MPa, and the drying time is 4h to obtain a modified aerogel thermal insulation composite material;
[0058] 7) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 260° C. for 2 h to remove impurities, thereby obtaining a wave-transmitting thermal insulation aerogel material;
[0059] 8) Surface modification: PFDTES was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L; the wave-transmitting heat-insulating aerogel material prepared in step 6) was then placed in a container and placed in a vacuum impregnation tank, and the surface modifier was slowly pumped into the container at 40°C and -0.1 MPa vacuum to fully impregnate the material, and maintained for 12 hours; after taking out, heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material.
[0060] The obtained reusable wave-transmitting heat-insulating aerogel material has the following properties:
[0061] The reusable wave-transmitting and heat-insulating aerogel material was heat-treated 10 times in a muffle furnace at 500°C for 2h, with a mass loss rate of 2.1%, a contact angle of 150.3°, and a mass moisture absorption rate of 1.90%. It still has excellent wave-transmitting and heat-insulating properties. After moisture absorption, the dielectric constant is 2.1, the dielectric loss tangent is 0.004 (10GHz), and the thermal conductivity at room temperature is 0.020W / mK.
[0062] Embodiment 2:
[0063] A method for preparing a reusable wave-transmitting heat-insulating aerogel material comprises the following steps:
[0064] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1:0.5:4:10:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0065] The silicon source is selected from tetraethyl orthosilicate;
[0066] The hydrophobic agent is selected from PTES;
[0067] The alcohol substance is selected from ethanol;
[0068] The acid catalyst is selected from hydrochloric acid;
[0069] The alkaline catalyst is selected from aqueous ammonia;
[0070] Sol preparation is carried out in two steps:
[0071] A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 mass of ethanol, 1 / 2 mass of deionized water and hydrochloric acid, mix and stir evenly to obtain solution ①, add ethyl orthosilicate dropwise to solution ①, stir and hydrolyze at 40℃ for 2h to obtain solution ②;
[0072] B. According to the molar ratio of the sol, 1 / 3 of the mass of ethanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0073] 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain 0.005 mol / L Ce(NO 3 ) 3 solution; finally, stirring was continued for 5 h in a water bath at 30°C to obtain a modifier;
[0074] 2) Preform molding: Preform the inorganic fiber at 0.25g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0075] The inorganic fiber is selected from quartz fiber;
[0076] 3) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box at -0.06MPa and -5°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 1-4h to fully impregnate it;
[0077] 4) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 48 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0078] 5) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 280°C, the pressure is 12MPa, and the drying time is 8h to obtain a modified aerogel thermal insulation composite material;
[0079] 6) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 300° C. for 2 h to remove impurities, thereby obtaining a wave-transmitting thermal insulation aerogel material;
[0080] 7) Surface modification: PFDTES was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L; the wave-transmitting heat-insulating aerogel material prepared in step 6) was then placed in a container and placed in a vacuum impregnation tank, and the surface modifier was slowly pumped into the container at 40°C and -0.1 MPa vacuum to fully impregnate the material, and maintained for 12 hours; after taking out, heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material.
[0081] The obtained reusable wave-transmitting heat-insulating aerogel material has the following properties:
[0082] The reusable wave-transmitting and heat-insulating aerogel material was heat-treated 10 times in a muffle furnace at 500°C for 2h, with a mass loss rate of 1.8%, a contact angle of 160.5°, and a mass moisture absorption rate of 0.98%. It still has excellent wave-transmitting and heat-insulating properties. After moisture absorption, the dielectric constant is 1.5, the dielectric loss tangent is 0.008 (10GHz), and the thermal conductivity at room temperature is 0.030W / mK.
[0083] Embodiment 3:
[0084] A method for preparing a reusable wave-transmitting heat-insulating aerogel material comprises the following steps:
[0085] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1:0.5:4:15:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0086] The silicon source is selected from tetraethyl orthosilicate;
[0087] The hydrophobic agent is selected from MTEOS;
[0088] The alcohol substance is selected from ethanol;
[0089] The acid catalyst is selected from nitric acid;
[0090] The alkaline catalyst is selected from aqueous ammonia;
[0091] Sol preparation is carried out in two steps:
[0092] A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 mass of ethanol, 1 / 2 mass of deionized water and nitric acid, mix and stir evenly to obtain solution ①, add ethyl orthosilicate dropwise to solution ①, stir and hydrolyze at 50°C for 4h to obtain solution ②;
[0093] B. According to the molar ratio of the sol, 1 / 3 of the mass of ethanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0094] 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain 0.005 mol / L Ce(NO 3 ) 3 solution; finally, stirring was continued for 5 h in a water bath at 30°C to obtain a modifier;
[0095] 3) Preform molding: The inorganic fiber is pressed at 0.22g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0096] The inorganic fiber is selected from basalt fiber;
[0097] 4) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box under -0.1MPa and -5°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 1-4h to fully impregnate it;
[0098] 5) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 48 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0099] 6) Supercritical drying: the aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 280°C, the pressure is 12MPa, and the drying time is 8h to obtain a modified aerogel thermal insulation composite material;
[0100] 7) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 300° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material;
[0101] 8) Surface modification: PFDTES was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L; the wave-transmitting heat-insulating aerogel material prepared in step 6) was then placed in a container and placed in a vacuum impregnation tank, and the surface modifier was slowly pumped into the container at 40°C and -0.1 MPa vacuum to fully impregnate the material, and maintained for 12 hours; after taking out, heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material.
[0102] The obtained reusable wave-transmitting heat-insulating aerogel material has the following properties:
[0103] The reusable wave-transmitting and heat-insulating aerogel material was heat-treated 10 times in a muffle furnace at 500°C for 2h, with a mass loss rate of 1.56%, a contact angle of 159.8°, and a mass moisture absorption rate of 1.01%. It still has excellent wave-transmitting and heat-insulating properties. After moisture absorption, the dielectric constant is 1.3, the dielectric loss tangent is 0.006 (10GHz), and the thermal conductivity at room temperature is 0.022W / mK.
[0104] Figure 2 This is a picture of the hydrophobic surface of the reusable wave-transmitting and heat-insulating aerogel material prepared in Example 3 after heat treatment 10 times in a muffle furnace at 500° C. for 2 h.
[0105] Embodiment 4:
[0106] A method for preparing a reusable wave-transmitting heat-insulating aerogel material comprises the following steps:
[0107] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1:1:3:20:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0108] The silicon source is selected from tetraethyl orthosilicate;
[0109] The hydrophobic agent is selected from MTEOS;
[0110] The alcohol substance is selected from isopropanol;
[0111] The acid catalyst is selected from hydrochloric acid;
[0112] The alkaline catalyst is selected from aqueous ammonia;
[0113] Sol preparation is carried out in two steps:
[0114] A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 mass of isopropanol, 1 / 2 mass of deionized water and hydrochloric acid, mix and stir evenly to obtain solution ①, add ethyl orthosilicate dropwise to solution ①, stir and hydrolyze at 50°C for 4h to obtain solution ②;
[0115] B. According to the molar ratio of the sol, 1 / 3 of the mass of isopropanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0116] 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain 0.005 mol / L Ce(NO 3 ) 3 solution; finally, stirring was continued for 5 h in a water bath at 30°C to obtain a modifier;
[0117] 3) Preform molding: The inorganic fiber is pressed at 0.18g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0118] The inorganic fiber is selected from basalt fiber;
[0119] 4) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box at -0.1MPa and -5°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 1 hour to fully impregnate it;
[0120] 5) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 48 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0121] 6) Supercritical drying: the aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 260°C, the pressure is 8MPa, and the drying time is 4h; the modified aerogel thermal insulation composite material is obtained;
[0122] 7) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 300° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material;
[0123] 8) Surface modification: PFDTES was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L; the wave-transmitting heat-insulating aerogel material prepared in step 6) was then placed in a container and placed in a vacuum impregnation tank, and the surface modifier was slowly pumped into the container at 40°C and -0.1 MPa vacuum to fully impregnate the material, and maintained for 12 hours; after taking out, heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material.
[0124] The obtained reusable wave-transmitting heat-insulating aerogel material has the following properties:
[0125] The reusable wave-transmitting and heat-insulating aerogel material was heat-treated 10 times in a muffle furnace at 500°C for 2h, with a mass loss rate of 3.85%, a contact angle of 140.6°, and a mass moisture absorption rate of 1.26%. It still has excellent wave-transmitting and heat-insulating properties. After moisture absorption, the dielectric constant is 1.8, the dielectric loss tangent is 0.009 (10GHz), and the thermal conductivity at room temperature is 0.020W / mK.
[0126] Comparative Example 1:
[0127] The existing process for preparing hydrophobic aerogel, compared with Example 3, does not adopt the in-situ method + surface modification method to prepare the reusable wave-transmitting heat-insulating aerogel material. The steps are as follows:
[0128] 1) Sol preparation: Silicon source, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1:4:5:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0129] The silicon source is selected from tetraethyl orthosilicate;
[0130] The alcohol substance is selected from ethanol;
[0131] The acid catalyst is selected from nitric acid;
[0132] The alkaline catalyst is selected from aqueous ammonia;
[0133] Sol preparation is carried out in two steps:
[0134] A. According to the molar ratio of the sol, 2 / 3 of the mass of ethanol, 1 / 2 of the mass of deionized water and nitric acid were mixed and stirred evenly to obtain solution ①, and ethyl orthosilicate was added dropwise to solution ①, and stirred and hydrolyzed at 40℃ for 2h to obtain solution ②;
[0135] B. According to the molar ratio of the sol, 1 / 3 of the mass of ethanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0136] 2) Preform molding: The inorganic fiber is pressed at 0.22g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0137] The inorganic fiber is selected from basalt fiber;
[0138] 3) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box at -0.1MPa and -5°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 2 hours to fully impregnate it;
[0139] 4) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 48 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0140] 5) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 280°C, the pressure is 12MPa, and the drying time is 8h to obtain a modified aerogel thermal insulation composite material;
[0141] 6) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 260° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material;
[0142] The obtained aerogel wave-transmitting heat-insulating material has the following properties:
[0143] The reusable wave-transmitting and heat-insulating aerogel material was placed in a muffle furnace for heat treatment at 500°C for 2h for 10 times, and the mass loss rate was 0.56%, the contact angle was 0°, the mass moisture absorption rate was 30.6%, and the wave-transmitting and heat-insulating performance was significantly reduced. After moisture absorption, the dielectric constant was greater than 10, the dielectric loss tangent was 0.018 (10GHz), and the thermal conductivity at room temperature was 0.223W / mK.
[0144] Figure 3 This is a picture of the surface of the wave-transmitting and heat-insulating aerogel material prepared in Comparative Example 1, which was heat-treated 10 times in a muffle furnace at 500° C. for 2 hours.
[0145] Comparative Example 2:
[0146] The preparation process of alumina aerogel is different from that of Example 3 in that no inorganic metal oxide cerium oxide is added and no surface modification method is used to improve the high temperature resistance of the aerogel material. The steps are as follows:
[0147] 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1:0.5:4:5:1.8×10 -3 :3.6×10 -2 Prepare sol;
[0148] The silicon source is selected from tetraethyl orthosilicate;
[0149] The hydrophobic agent is selected from MTEOS;
[0150] The alcohol substance is selected from ethanol;
[0151] The acid catalyst is selected from nitric acid;
[0152] The alkaline catalyst is selected from aqueous ammonia;
[0153] Sol preparation is carried out in two steps:
[0154] A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 mass of ethanol, 1 / 2 mass of deionized water and nitric acid, mix and stir evenly to obtain solution ①, add ethyl orthosilicate dropwise to solution ①, stir and hydrolyze at 40℃-50℃ for 2h-4h to obtain solution ②;
[0155] B. According to the molar ratio of the sol, 1 / 3 of the mass of ethanol, the remaining deionized water and ammonia water are mixed to form solution ③, and solution ③ is added dropwise to solution ② to obtain a solution containing SiO 2 Sols of nanoparticles;
[0156] 2) Preform molding: The inorganic fiber is pressed at 0.22g / cm 3The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation;
[0157] The inorganic fiber is selected from basalt fiber;
[0158] 3) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; evenly mix the sol in step 1) and the modifier in step 2) and slowly pump them into the plastic box at -0.1MPa and -5°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 1-4h to fully impregnate it;
[0159] 4) Gel and aging treatment: After the impregnation, the glue box is sealed and placed in a 40°C environment to wait for gelation. After gelation, an alcohol substance is added to the glue box to protect the gel surface from cracking. After sealing, the glue box is kept in a 40°C environment for aging for 48 hours; the alcohol substance is the same as the alcohol substance used in the sol preparation in step 1);
[0160] 5) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 280°C, the pressure is 12MPa, and the drying time is 8h to obtain a modified aerogel thermal insulation composite material;
[0161] 6) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 300° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material;
[0162] The reusable wave-transmitting heat-insulating aerogel material was heat-treated 10 times in a muffle furnace at 500°C for 2h, and the mass loss rate was 2.34%, the contact angle was 109.8°, the mass moisture absorption rate was 12.4%, the hydrophobicity decreased, the dielectric constant was greater than 10 after moisture absorption, the dielectric loss tangent was 0.012 (10GHz), and the thermal conductivity at room temperature was 0.075W / mK.
[0163] The results show that:
[0164] 1. By comparing Example 3 with Comparative Example 1, it is shown that the wave-transmitting and heat-insulating aerogel composite material prepared by the in-situ method + surface modification method has excellent reusability, and after repeated heat treatment at 500°C for 2h, it still has super hydrophobicity, low dielectric constant and dielectric loss, and low thermal conductivity.
[0165] 2. By comparing Example 3 with Comparative Example 2, it is shown that the wave-transmitting and heat-insulating aerogel composite material prepared by the in-situ method + surface modification method has better high temperature resistance than that prepared by the in-situ method alone, and the addition of the inorganic oxide cerium oxide and the modification of PFDTES make the material's high-temperature reusability better.
[0166] The above are only preferred implementations of the present invention. The protection scope of the present invention is not limited to the above embodiments. Various process schemes that are not substantially different from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a reusable wave-transmitting heat-insulating aerogel material, characterized in that: The following steps are involved: 1) Sol preparation: Silicon source, hydrophobic agent, alcohol, deionized water, acid catalyst, and base catalyst are mixed in a molar ratio of 1: (0.25-1): (3-4): (5-20): 1.8×10 -3 :3.6×10 -2 Prepare sol; The silicon source is selected from one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate and isopropyl orthosilicate; The hydrophobic agent is selected from one of phenyltrimethoxysilane, phenyltriethoxysilane and methyltriethoxysilane; The alcohol substance is selected from one of methanol, ethanol, isopropanol, n-butanol, sec-butanol and tert-butanol; The acid catalyst is selected from hydrochloric acid, nitric acid and sulfuric acid; The alkaline catalyst is selected from aqueous ammonia; Sol preparation is carried out in two steps: A. According to the molar ratio of the sol configuration, take the whole mass of the hydrophobic agent, 2 / 3 of the mass of the alcohol substance, 1 / 2 of the mass of the deionized water and the acid catalyst, mix and stir evenly to obtain solution ①, add the silicon source dropwise to solution ①, stir and hydrolyze at 40℃-50℃ for 2h-4h to obtain solution ②; B. According to the molar ratio of the sol configuration, 1 / 3 of the alcohol substance by mass, the remaining deionized water and the alkaline catalyst are mixed to form a solution ③, and the solution ③ is added dropwise to the solution ② to obtain a sol containing SiO2 nanoparticles; 2) Prepare the modifier: dissolve 0.01 mol glucose and 0.015 mol acrylic acid in 80 ml deionized water under strong stirring; continue to add cerium nitrate hexahydrate under stirring to obtain a Ce(NO3)3 solution with a concentration of 0.003-0.006 mol / L; finally, continue stirring in a 30°C water bath for 5 hours to obtain the modifier; 3) Preform molding: Preform the inorganic fiber at 0.1-0.25g / cm 3 The fiber density is molded to obtain a preform, and the preform is placed in a glue box to wait for impregnation; The inorganic fiber is selected from one of glass fiber, basalt fiber and quartz fiber; 4) Impregnation: Place the preformed plastic box in the previous step into a vacuum impregnation tank; mix the SiO2 nanoparticle sol obtained in step 1) and the modifier obtained in step 2) evenly, and then slowly pump them into the plastic box at -0.06 to -0.1 MPa and -5 to 0°C. When the sol liquid level submerges the preform, maintain the pressure in the vacuum impregnation tank for 1 to 4 hours to fully impregnate it; 5) Gel and aging treatment: seal the glue box after impregnation and place it in a 40°C environment to wait for gelation. After gelation, add alcohol substances to the glue box to protect the gel surface from cracking. After sealing, keep it in a 40°C environment for aging for 12-48 hours; The alcohol substance is the same as the alcohol substance used in the sol preparation in step 1); 6) Supercritical drying: The aged plastic box is placed in a supercritical drying kettle for drying, the supercritical temperature is 260-280°C, the pressure is 8-12MPa, and the drying time is 4-8h to obtain a modified aerogel thermal insulation composite material; 7) Post-heat treatment: placing the prepared modified aerogel thermal insulation composite material into an oven and heat treating it at 260-300° C. for 2 h to obtain a wave-transmitting thermal insulation aerogel material; 8) Surface modification: 1H,1H,2H,2H-perfluorodecyltriethoxysilane was added to hexane and stirred for 10 min to obtain a surface modifier with a concentration of 0.01 mol / L; Then, the wave-transmitting heat-insulating aerogel material prepared in step 6) is placed in a container and placed in a vacuum impregnation tank. The surface modifier is slowly pumped into the container at 40°C and -0.1MPa vacuum to fully impregnate the wave-transmitting heat-insulating aerogel material, and the surface modifier is kept for 12 hours. After being taken out, the material is heat-treated in a muffle furnace at 120°C for 24 hours to obtain a reusable wave-transmitting heat-insulating aerogel material. The reusable wave-transmitting heat-insulating aerogel material is placed in a muffle furnace at 500°C and 2h. After 10 times of medium heat treatment, it still has excellent hydrophobic effect and wave-transmitting and heat-insulating performance, with a mass loss rate of 1.56-3.85%; a contact angle of 140.6°-160.5°; a mass moisture absorption rate of 0.98-1.90%; and still has excellent wave-transmitting and heat-insulating performance; the dielectric constant after moisture absorption is 1.3-2.1; the dielectric loss tangent value is 0.004-0.009, 10GHz; the thermal conductivity at room temperature is 0.020-0.030W / mK.
2. The method for preparing a reusable wave-transmitting heat-insulating aerogel material according to claim 1, characterized in that: The strong stirring condition in step 2) is at a rotation speed of 800-1000 rpm; the stirring condition is at a rotation speed of 100-200 rpm; the continuous stirring is at a rotation speed of 100-200 rpm.
3. A reusable wave-transmitting heat-insulating aerogel material, characterized by: The reusable wave-transmitting heat-insulating aerogel material is prepared by the preparation method of any one of claims 1-2. The reusable wave-transmitting heat-insulating aerogel material is placed in a muffle furnace at 500°C for 2h for heat treatment 10 times, and still has excellent hydrophobic effect and wave-transmitting heat-insulating performance, with a mass loss rate of 1.56-3.85%; a contact angle of 140.6°-160.5°; a mass moisture absorption rate of 0.98-1.90%; a dielectric constant of 1.3-2.1 after moisture absorption; a dielectric loss tangent of 0.004-0.009, 10GHz; and a thermal conductivity of 0.020-0.030W / mK at room temperature.
Citation Information
Patent Citations
Silicon dioxide aerogel composite material and preparation method and application thereof
CN109336545A
Normal-pressure preparation method of rare-earth oxide doped cerium oxide aerogel
CN112058314A
Wave-transmitting, efficient and heat-insulating aerogel composite material and preparation method thereof
CN112851292A
Preparation method of aerogel material and application of aerogel material
CN114261986A
Silicon-based monobasic or multibasic oxide aerogel material and preparation method therefor
WO2015192731A1
Cited By
Aerogel composite material capable of being repeatedly used and packaged under high-temperature condition and preparation method of aerogel composite material
CN119633702A