MnO-coated core-shell structure fine grain energy storage dielectric ceramic material, preparation method and application of MnO-coated core-shell structure fine grain energy storage dielectric ceramic material

MnO-coated Ba0.99Bi0.01TiO3 ceramic materials are prepared through chemical precipitation and liquid coating methods, which solves the problems of insufficient dielectric performance and energy storage density in the existing technology and achieves high energy storage density and low dielectric loss. The "core-shell" structure ceramic material is suitable for applications such as multilayer ceramic capacitors.

CN118754644AActive Publication Date: 2024-10-11BAOJI UNIV OF ARTS & SCI

Patent Information

Application Number
CN202410857004.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

It is difficult to prepare MnO-coated "core-shell" structure fine-grain energy storage dielectric ceramic materials with high energy storage density and optimized dielectric properties using existing technology, and there is a lack of effective preparation methods to meet the needs of multilayer ceramic capacitors.

Method used

Ba0.99Bi0.01TiO3 micro-nano powder was prepared by chemical precipitation method, and MnO was evenly coated on the surface of Ba0.99Bi0.01TiO3 by liquid phase coating method, and then sintered to prepare Ba0.99Bi0.01TiO3@xMnO dielectric ceramic material , adjust the MnO content to optimize material properties.

Benefits of technology

The dielectric constant reaches 3610, the dielectric loss is small, and the discharge energy storage density reaches 0.26J/cm3. It is suitable for ceramic energy storage capacitors with large capacity and ultra-thin dielectric layer, and improves the energy storage density and resistivity of the material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754644A_ABST
    Figure CN118754644A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electronic ceramic energy storage capacitor materials, and particularly relates to a MnO-coated'core-shell 'structure fine-grain energy storage dielectric ceramic material, a preparation method and application of the MnO-coated'core-shell' structure fine-grain energy storage dielectric ceramic material. According to the dielectric ceramic material BBT, due to the good dielectric property, micro-nano BBT powder particles are selected as a core part material, the ion radiuses of Mn < 2 + > and Ti < 4 + > are close, manganese occupies the titanium site in barium titanate more easily in the substitution process, when high-valence titanium is replaced by low-valence manganese, defects can be formed in ceramic crystals, and therefore the dielectric constant is reduced; mn < 3 + > and Mn < 4 + > can effectively capture electrons, so that the carrier concentration in the dielectric ceramic material is reduced, the dielectric ceramic material has low dielectric loss, and the resistivity of the dielectric ceramic material is improved; based on the design of the microstructure, the microstructure of the ceramic can be optimized, the dielectric loss is reduced, and the energy storage density of the ceramic is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic ceramic energy storage capacitor materials, and specifically relates to a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, a preparation method and an application thereof. Background Art

[0002] Barium titanate (BaTiO3) has been proven to be an excellent ferroelectric ceramic; the ferroelectricity of BaTiO3 originates from the spontaneous polarization of the crystal below its transition temperature; due to its advantages such as large dielectric constant, extremely low dielectric loss, small leakage current, and small electro-optic coefficient, it has potential application prospects in various electronic devices such as multilayer ceramic capacitors, positive temperature coefficient (PTC) resistors, optoelectronic devices, piezoelectric sensors, and energy storage systems. Bi-containing compounds are favored by researchers because they have a low melting point and are easily volatile during high-temperature sintering, which can promote the sintering of ceramics without deteriorating the dielectric properties of ceramics.

[0003] Ur et al. prepared 0.94BT-0.06BMC+xwt.%SiO2 ceramics by solid phase sintering method; and 0.94BT-0.06BMC+1wt.%SiO2 ceramic samples have good energy storage density (W rec =1.035J / cm -3 ) and higher dielectric breakdown strength (BDS = 285 kV / cm -1 ), indicating that an appropriate amount of SiO2 doped BT-BMC ceramics can improve the insulation properties of ceramics, improve the BDS of ceramics, and enable them to be used in capacitors. (Ur, Manan A, Khan MA, et al. The effects of SiO2 addition on the phase, microstructure, dielectric, and energy storage properties of BaTiO3-based ceramics [J]. Materials Science & Engineering, B. Solid-State Materials for Advanced Technology, 2023.). Lai et al. prepared MgO-coated BT powder by chemical precipitation and obtained BaTiO3@xMgO (x = 0-7 mol%) ceramics with a "core-shell" structure. Compared with the solid phase method, the wet chemical method can more effectively modify the powder surface and easily form a "core-shell" structure, which is conducive to the formation of fine-grained ceramics with good stability at high temperatures. Due to Mg 2+ Ion substitution Ti 4+ Ion, Mg 2+The solid solubility limit of ions is 0.8 mol%; when x ≥ 0.8 mol%, Mg 2+ The ions stay at the grain boundaries, forming a secondary phase, and a core-shell structure is obtained through the Mg gradient distribution, indicating that the formed "core-shell" structure has stable dielectric properties. (Lai X, Hao H, Liu Z, et al. Structure and dielectric properties of MgO-coated BaTiO3 ceramics [J]. Journal of Materials Science: Materials in Electronics, 2020, 31 (11).). Shalu et al. synthesized lead-free, environmentally friendly polycrystalline BSMT nanopowders by sol-gel method, and doped different contents of Mn into Ba 0.7 Sr 0.3 In TiO3, doping with an appropriate amount of Mn can promote the mass transfer process, but at higher solution concentrations, Mn ions hinder the diffusion of other ions, resulting in a decrease in grain size; and the 2% Mn-doped sample has the highest dielectric constant and excellent ferroelectric properties. (Shalu S, Roy S, Mukherjee A. Effect of Mn-doping on the morphological and electrical properties of (Ba 0.7 Sr 0.3 )(Mn x Ti1 -x )O3 materials for energy storage application[J].Ceramics International, 2022(18):48.).

[0004] In order to further meet the needs of high energy storage density and miniaturization of "core-shell" structural materials, there is an urgent need for a MnO-coated "core-shell" structured fine-grained energy storage dielectric ceramic material to optimize the dielectric properties and energy storage performance of the ceramic material; and there is an urgent need for a preparation method of a MnO-coated "core-shell" structured fine-grained energy storage dielectric ceramic material, thereby laying the foundation for the preparation of multilayer ceramic capacitors.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to overcome the disadvantages of the prior art and provide a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, a preparation method and an application thereof.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] On the one hand, the present invention provides a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, comprising Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder, the Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder includes a "core" part and a "shell" part, and the "core" part is made of Ba 0.99 B i0.01 TiO3, the "shell" material is MnO;

[0009] Wherein, 0≤x≤1, and x can be adaptively adjusted according to actual preparation requirements, and optional values ​​are 0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%, etc., which are not listed one by one.

[0010] On the other hand, the present invention provides a method for preparing a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, firstly preparing a monodisperse Ba 0.99 B i0.01 TiO3 micro-nano powder, and then prepared monodisperse MnO-coated Ba by liquid phase coating method 0.99 B i0.01 TiO3@xMnO micro-nano powder was finally sintered to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

[0011] The specific steps are as follows:

[0012] Step 1, add the TiCl4 solution dropwise into a 4-8 mol / L NaOH solution, place in a water bath at a temperature of 10-40°C, and stir thoroughly for 0.5-2h;

[0013] Step 2: prepare aqueous solutions of bismuth compound and barium compound respectively according to the stoichiometric ratio, then slowly add the above solutions respectively, and stir continuously, the reaction temperature is 10-40° C., and the stirring reaction time is 0.5-2 h;

[0014] Step 3: Place the obtained solution in a water bath at a temperature of 80-100°C and continue stirring for 4-6 hours, then filter and dry in an oven at 80-100°C to obtain Ba 0.99 Bi 0.01 TiO3 powder;

[0015] Step 4: Ba 0.99 Bi 0.01TiO3 powder was ultrasonically dispersed in deionized water and ethanol to obtain Ba 0.99 Bi 0.01 TiO3 suspension, then add 30% ammonia solution, and adjust the pH to 9-11; the mass ratio of deionized water to ethanol is (2:3);

[0016] Step 5: prepare a manganese acetate solution using a stoichiometric ratio, then add it dropwise to the above solution, and use mechanical stirring at a speed of 60-80 R / min to mix it evenly, so that the MnO generated by the reaction is evenly coated on the Ba 0.99 Bi 0.01 TiO3 particle surface;

[0017] Step 6: After the precipitation is complete, the suspension is aged for a certain period of time, and then the suspension is filtered and washed several times, and then dried in an oven at 80-100°C to obtain micro-nano powders, and the obtained micro-nano powders are calcined in air at 700-900°C for 1-2h, and Ba is obtained after cooling. 0.99 Bi 0.01 TiO3@xMnO micro-nano dielectric powder;

[0018] Step 7: Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano medium powder was ground with PVA and glycerol for granulation. After granulation, it was pressed into sheets by a mold at 8-10MPa and sintered at 1220-1260℃ for 2-4h to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

[0019] Specifically, the Ba obtained in step 3 0.99 Bi 0.01 TiO3 powder is a monodisperse micro-nano powder with a particle size of 50-500nm.

[0020] Specifically, the Ba obtained in step 6 0.99 Bi 0.01 The ceramic grains of TiO3@xMnO micro-nano dielectric powder are about 100-500nm.

[0021] Specifically, the MnO is coated on the monodispersed Ba 0.99 Bi 0.01 TiO3 particle surface.

[0022] Specifically, in step 7, the Ba 0.99 Bi 0.01 After being pressed, TiO3@xMnO micro-nano powder is sintered at 1220-1260°C for 2-6 hours to produce dielectric ceramic material.

[0023] Specifically, the Ba prepared in step 7 0.99 Bi 0.01 The discharge energy storage density of TiO3@xMnO dielectric ceramic materials is 0.09-0.26 J / cm 3 .

[0024] On the other hand, the present invention provides a Ba prepared by the preparation method as described above. 0.99 Bi 0.01 Application of TiO3@xMnO dielectric ceramic materials, the Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials are used in applications including but not limited to the preparation of multilayer ceramic capacitors, positive temperature coefficient (PTC) resistors, optoelectronic devices, piezoelectric sensors, and energy storage systems.

[0025] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0026] The present invention designs a microstructure-controllable fine-grained energy storage dielectric ceramic material BBT. Since BBT has excellent dielectric properties, we choose micro-nano BBT powder particles as the "core" material, and Mn 2+ and Ti 4+ The ionic radius of Mn is close to that of Ti in barium titanate. When low-valent manganese replaces high-valent titanium, defects will be formed in the ceramic crystal, thereby reducing the dielectric constant. 3+ and Mn 4+ It can effectively capture electrons, thereby reducing the carrier concentration in the dielectric ceramic material, making the dielectric ceramic material have low dielectric loss, and improving the resistivity of the dielectric ceramic material; based on the design of this microstructure, it can optimize the ceramic micromorphology, reduce dielectric loss, and improve the energy storage density of the ceramic.

[0027] Further, the Ba prepared by the present invention 0.99 Bi 0.01 TiO3 micro-nano powder material has the characteristics of particle size of 50-500nm and good dispersibility.

[0028] Furthermore, the fine-grained energy storage dielectric ceramic material prepared by the present invention has a discharge energy storage density of 0.26 J / cm 3 , the dielectric constant reaches 3610, and the dielectric loss is small.

[0029] Furthermore, the ceramic grain size prepared by the present invention is about 100-500nm, the particle size is uniform, and the reliability is strong, and it is suitable for producing ceramic energy storage capacitors with large capacity and ultra-thin dielectric layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0032] Figure 1 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 SEM image of TiO3@xMnO dielectric powder sample;

[0033] Figure 2 #1-3Ba in Example 1 0.99 Bi 0.01 TEM image of TiO3@0.4mol%MnO dielectric powder sample;

[0034] Figure 3 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 SEM image of TiO3@xMnO dielectric ceramic sample;

[0035] Figure 4 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 XRD pattern of TiO3@xMnO dielectric powder;

[0036] Figure 5 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 XRD pattern of TiO3@xMnO dielectric ceramic sample;

[0037] Figure 6 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 Dielectric constant diagram of TiO3@xMnO dielectric ceramic samples;

[0038] Figure 7For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 Characteristic curve of dielectric loss of TiO3@xMnO dielectric ceramic sample changing with temperature;

[0039] Figure 8 For #1-1, #1-2, #1-3, #1-4, #1-5, #1-6Ba in Example 1 0.99 Bi 0.01 Hysteresis loop diagram of TiO3@xMnO dielectric ceramic sample before breakdown;

[0040] Fig. 9 For #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba in Example 2 0.99 Bi 0.01 SEM image of TiO3@xMnO dielectric ceramic sample;

[0041] Fig.10 For #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba in Example 2 0.99 Bi 0.01 XRD pattern of TiO3@xMnO dielectric ceramic sample;

[0042] Fig.11 For #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba in Example 2 0.99 Bi 0.01 Dielectric constant diagram of TiO3@xMnO dielectric ceramic samples;

[0043] Fig.12 For #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba in Example 2 0.99 Bi 0.01 Characteristic curve of dielectric loss of TiO3@xMnO dielectric ceramic sample changing with temperature;

[0044] Fig.13 For #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba in Example 2 0.99 Bi 0.01 Hysteresis loop diagram of TiO3@xMnO dielectric ceramic sample before breakdown. DETAILED DESCRIPTION

[0045] Here, exemplary embodiments will be described in detail, and examples thereof are shown in the accompanying drawings. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.

[0046] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0047] The present invention provides a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, which comprises Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder is made, the Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder includes a "core" part and a "shell" part, and the "core" part is made of Ba 0.99 B i0.01 TiO3, the "shell" material is MnO;

[0048] Wherein, 0≤x≤1, and x can be adaptively adjusted according to actual preparation requirements, and optional values ​​are 0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%, etc., which are not listed one by one.

[0049] On the other hand, the present invention provides a method for preparing a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, firstly preparing a monodisperse Ba 0.99 B i0.01 TiO3 micro-nano powder, and then prepared monodisperse MnO-coated Ba by liquid phase coating method 0.99 B i0.01 TiO3@xMnO micro-nano powder was finally sintered to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

[0050] The specific steps are as follows:

[0051] Step 1, add the TiCl4 solution dropwise into a 4-8 mol / L NaOH solution, place in a water bath at a temperature of 10-40°C, and stir thoroughly for 0.5-2h;

[0052] Step 2: prepare aqueous solutions of bismuth compound and barium compound respectively according to the stoichiometric ratio, then slowly add the above solutions respectively, and stir continuously, the reaction temperature is 10-40° C., and the stirring reaction time is 0.5-2 h;

[0053] Step 3: Place the obtained solution in a water bath at a temperature of 80-100°C and continue stirring for 4-6 hours, then filter and dry in an oven at 80-100°C to obtain Ba 0.99 Bi 0.01 TiO3 powder;

[0054] Step 4: Ba 0.99 Bi 0.01 TiO3 powder was ultrasonically dispersed in deionized water and ethanol to obtain Ba 0.99 Bi 0.01 TiO3 suspension, then add 30% ammonia solution, and adjust the pH to 9-11; the mass ratio of deionized water to ethanol is 2:3;

[0055] Step 5: prepare a manganese acetate solution using a stoichiometric ratio, then add it dropwise to the above solution, and use mechanical stirring at a speed of 60-80 R / min to mix it evenly, so that the MnO generated by the reaction is evenly coated on the Ba 0.99 Bi 0.01 TiO3 particle surface;

[0056] Step 6: After the precipitation is complete, the suspension is aged for a certain period of time, and then the suspension is filtered and washed several times, and then dried in an oven at a temperature of 80-100°C to obtain micro-nano powders, and the obtained micro-nano powders are calcined in air at 700-900°C for 1-2h, and Ba is obtained after cooling. 0.99 Bi 0.01 TiO3@xMnO micro-nano dielectric powder;

[0057] Step 7: Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano medium powder was ground with PVA and glycerol for granulation. After granulation, it was pressed into sheets by a mold at 8MPa and sintered at 1220-1260℃ for 2-4h to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

[0058] Specifically, the Ba obtained in step 3 0.99 Bi 0.01 TiO3 powder is a monodisperse micro-nano powder with a particle size of 50-500nm.

[0059] Specifically, the Ba obtained in step 6 0.99 Bi 0.01 The ceramic grains of TiO3@xMnO micro-nano dielectric powder are about 100-500nm.

[0060] Specifically, the MnO is coated on the monodispersed Ba0.99 Bi 0.01 TiO3 particle surface.

[0061] Specifically, in step 7, the Ba 0.99 Bi 0.01 After being pressed, TiO3@xMnO micro-nano powder is sintered at 1220-1260°C for 2-6 hours to produce dielectric ceramic material.

[0062] Specifically, the Ba prepared in step 7 0.99 Bi 0.01 The discharge energy storage density of TiO3@xMnO dielectric ceramic materials is 0.04-0.25J / cm 3 .

[0063] In order to further verify the preparation method of MnO-coated "core-shell" structured fine-grained energy storage dielectric ceramic materials, the prepared Ba 0.99 Bi 0.01 The properties of TiO3@xMnO dielectric ceramic materials, the present invention also provides the following embodiments:

[0064] Example 1

[0065] Preparation of Ba 0.99 Bi 0.01 TiO3@xMnO powder and dielectric ceramic materials thereof, wherein x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%, and the corresponding sample numbers are #1-1, #1-2, #1-3, #1-4, #1-5, #1-6, respectively; Ba was prepared in this embodiment 0.99 Bi 0.01 The specific steps of TiO3@xMnO powder and its dielectric ceramic materials are as follows:

[0066] Step 1, at a water bath temperature of 30°C, slowly drop the TiCl4 solution into a 6 mol / L NaOH solution, and fully stir for 0.5h; slowly add the aqueous solutions of bismuth compound and barium compound respectively according to the stoichiometric ratio, and stir continuously, the reaction temperature is 30°C, and the reaction time is 0.5h; continue to stir the above solution at a water bath temperature of 90°C for 4h, wash, and dry in an oven at 80°C to obtain Ba 0.99 Bi 0.01 TiO3 powder;

[0067] Step 2, weigh 3.000g Ba 0.99 Bi 0.01 TiO3 powder was ultrasonically dispersed in 300 mL of deionized water for 30 min to obtain Ba 0.99 Bi 0.01The TiO3 suspension was adjusted to a pH above 9 with 30% ammonia water;

[0068] Step 3: Ba 0.99 Bi 0.01 The TiO3 suspension was transferred into a three-necked flask and stirred at room temperature at a stirring speed of 60 R / min, and the pH value was adjusted to above 10 with aqueous ammonia;

[0069] Step 4, weigh 0.0063g, 0.0125g, 0.0188g, 0.0251g, and 0.0314g of manganese acetate respectively, add the manganese acetate solution into a three-necked flask, use mechanical stirring at room temperature, the stirring speed is 60R / min, and stir thoroughly for 1h;

[0070] Step 5: After precipitation is complete, age for 24 hours, filter and wash several times, dry in an oven at 90°C, and then calcine at 800°C for 2 hours to obtain six kinds of Ba 0.99 Bi 0.01 TiO3@xMnO dielectric powder (x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%);

[0071] Step 6: Get the Ba 0.99 Bi 0.01 TiO3@xMnO medium powders (x = 0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%) were granulated and pressed into green discs with a diameter of 10 mm and a thickness of 1.5 mm at a pressure of 8 MPa, and sintered at 1250 ° C for 2 h to obtain six kinds of Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic samples (x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%).

[0072] See also Figure 1 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01 SEM image of TiO3@xMnO medium powder (SEM image is used to analyze the microscopic morphology of powder, all powders are photographed at 25000 times; the figure shows Ba 0.99 Bi 0.01 The TiO3@xMnO dielectric powders are uniform and well-dispersed spherical particles with average particle sizes of approximately 358, 382, ​​435, 402, 472, and 492 nm, respectively, which are conducive to the preparation of fine-grained dielectric ceramics. ).

[0073] See also Figure 2 As shown, the picture shows #1-3Ba 0.99Bi 0.01 TEM image of TiO3@0.4mol%MnO medium powder sample (TEM can see fine structures less than 0.2um that cannot be seen under an optical microscope. There is a uniform coating with a thickness of 19nm on the surface of BBT powder; the red manganese oxide outer layer can also be seen from the figure; however, the diffusion of Mn into the BBT "core" is very obvious, which is mainly related to the calcination process when preparing BBT@MnO powder. The increase in temperature will affect the diffusion of manganese. EDS analysis shows that the inner layer is mainly composed of Ba 2+ 、Bi 3+ 、Ti 4+ , O 2- ions, while the outer layer mainly contains Mn, indicating that MnO is uniformly coated on the surface of BBT ceramic powder. ).

[0074] See also Figure 3 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01 SEM images of TiO3@xMnO dielectric ceramic samples (SEM images are used to analyze the microscopic morphology of the ceramic surface. All Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic samples were all photographed at 13000 times. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2mol%, 0.4mol%, 0.6mol%, 0.8mol%, and 1.0mol% MnO dielectric ceramic samples, respectively. It can be seen from the figure that the ceramic structure is dense and the grain boundary is clear. After adding MnO, the ceramic grain size is reduced and accompanied by a small amount of holes; when x = 0.4mol%, the holes are the least; the reasons for the generation of holes can be attributed to: ① The sintering temperature is low and the internal reaction of the sample is not sufficient; ② The diffusion rate of manganese in BaTiO3-based materials is low, and the doped Mn 2+ and Mn 3+ The ions are enriched at the grain boundaries, thus inhibiting the densification between grains during sintering; ③ The doping of multivalent manganese ions contributes to the formation of titanium vacancies and oxygen vacancies, and the migration of oxygen vacancies reduces the density of the ceramic. ).

[0075] See also Figure 4 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01XRD diagram of TiO3@xMnO dielectric powder (XRD diagram is used to analyze the phase structure of powder, where the horizontal axis in the figure is the 2θ angle and the vertical axis is the relative intensity. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric powders, respectively; all dielectric powders are pure perovskite structure, no second phase appears, and no manganese oxide is detected; the specific reason is that the weak diffraction peak of a small amount of manganese oxide is covered by the diffraction curve of BBT.).

[0076] See also Figure 5 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01 XRD pattern of TiO3@xMnO dielectric ceramic sample; (XRD pattern is used to analyze the phase structure of ceramics, where the horizontal axis in the figure is the 2θ angle and the vertical axis is the relative intensity. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. Among them, the BBT particles have a pure perovskite structure and no second phase is observed. After coating with manganese, MnO, MnO2, and Mn3O4 peaks appeared in the XRD spectrum, which may be due to the thermal decomposition of manganese oxide, indicating that manganese oxide is successfully coated on Ba 0.99 Bi 0.01 TiO3 particles; from the magnified image, it can be seen that there is no obvious split peak in the magnified diffraction peak of the (200) crystal plane; however, there are signs of expansion and weak splitting, indicating that the ceramic may be in a state where tetragonal and cubic phases coexist; the diffraction pattern shows that the manganese oxide coating can slightly change the phase structure of the ceramic and promote the coexistence of multiple phases in the ceramic. ).

[0077] See also Figure 6 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01Dielectric constant diagram of TiO3@xMnO dielectric ceramic samples (the horizontal axis in the dielectric constant diagram is temperature, and the vertical axis is dielectric constant. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2mol%, 0.4mol%, 0.6mol%, 0.8mol%, and 1.0mol% MnO dielectric ceramic samples, respectively; in the figure, the dielectric constant first increases and then decreases with the increase of the MnO coating amount. When the MnO coating amount is 0.4mol%, the dielectric constant reaches a maximum value of 3610. When the MnO coating amount exceeds 0.4mol%, the dielectric constant decreases slightly; the increase in the dielectric constant of the manganese-doped sample is related to the Mn 3+ The electronic structure of Mn is related to the AB bond. 2+ To Mn 3+ The transition of will lead to orientation polarization, which is the electron exchange between these ions; the introduction of Mn may cause the TiO6 octahedron to deform, produce oxygen vacancies, and may also weaken the AB sublattice interaction, reduce the polarization resistance, and thus increase the dielectric constant; the reason for the decrease in the dielectric constant is that low-valent manganese replaces high-valent titanium, forming defects in the ceramic crystal, thereby reducing the dielectric constant. ).

[0078] See also Figure 7 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01 The characteristic curve of dielectric loss of TiO3@xMnO dielectric ceramic samples changing with temperature (the horizontal axis in the dielectric loss graph is temperature, and the vertical axis is dielectric loss. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2mol%, 0.4mol%, 0.6mol%, 0.8mol%, and 1.0mol% MnO dielectric ceramic samples, respectively. In the figure, the dielectric loss first decreases and then increases with the increase of the MnO coating amount. When the MnO coating amount is 0.4mol%, the dielectric loss is the smallest, which is 0.01; the reduction in dielectric loss is due to the Mn 3+ and Mn 4+ It can effectively capture electrons, thereby reducing the carrier density in the material; the ceramic containing 0.4mol% MnO obtained the largest dielectric constant (3610) and the lowest dielectric loss (0.01). ).

[0079] See also Figure 8 As shown, the figure shows six types of Ba #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 0.99 Bi 0.01Hysteresis loop diagram of TiO3@xMnO dielectric ceramic sample before breakdown (the horizontal axis in the figure is the ratio of electric field and ceramic thickness, and the vertical axis is polarization. In the figure, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. It can be seen from the figure that all ceramics show slender hysteresis loops, and the maximum polarization intensity (Pmax) first increases and then decreases. When the coating x=0.4 mol%, Pmax reaches the maximum value, and its energy storage density is calculated through the hysteresis loop.).

[0080] Its main energy storage property parameters are shown in Table 1:

[0081] Table 1 shows the energy storage performance parameters of dielectric ceramic samples #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6

[0082]

[0083] In the table, #1-1, #1-2, #1-3, #1-4, #1-5, and #1-6 are dielectric ceramic samples of MnO when x=0, 0.2mol%, 0.4mol%, 0.6mol%, 0.8mol, and 1.0mol%, respectively. It can be seen from the table that as the MnO content increases, the discharge energy density of the dielectric ceramic sample increases first and then decreases. When the coating layer x=0.4mol%, the discharge energy density reaches a maximum value of 0.26J / cm 3 , and achieves a higher energy storage efficiency of 76.5%.

[0084] Example 2

[0085] Preparation of Ba 0.99 Bi 0.01 TiO3@xMnO powder and dielectric ceramic materials thereof, wherein x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%, and the corresponding sample numbers are #2-1, #2-2, #2-3, #2-4, #2-5, #2-6, respectively; Ba was prepared in this embodiment 0.99 Bi 0.01 The specific steps of TiO3@xMnO powder and its dielectric ceramic materials are as follows:

[0086] Step 1, at a water bath temperature of 30°C, slowly drop the TiCl4 solution into a 6 mol / L NaOH solution, and fully stir for 0.5h; slowly add aqueous solutions of bismuth compound and barium compound respectively according to the stoichiometric ratio, and stir continuously, the reaction temperature is 40°C, and the reaction time is 1h; continue to stir the above solution at a water bath temperature of 100°C for 5h, wash, and dry in an oven at a temperature of 90°C to obtain Ba 0.99 Bi 0.01 TiO3 powder;

[0087] Step 2, weigh 3.000g Ba 0.99 Bi 0.01 TiO3 powder was ultrasonically dispersed in 300 mL of deionized water for 30 min to obtain Ba 0.99 Bi 0.01 TiO3 suspension was adjusted to pH above 9 with 30% ammonia water in five parallel groups;

[0088] Step 3: Ba 0.99 Bi 0.01 The TiO3 suspension was transferred into a three-necked flask and mechanically stirred at room temperature at a stirring speed of 80 R / min, and the pH value was adjusted to above 10 with aqueous ammonia;

[0089] Step 4, weigh 0.0063g, 0.0125g, 0.0188g, 0.0251g, and 0.0314g of manganese acetate respectively, add the manganese acetate solution into a three-necked flask, use mechanical stirring at room temperature, the stirring speed is 60R / min, and stir thoroughly for 1h;

[0090] Step 5: After precipitation is complete, age for 12 hours, filter, wash several times, dry in an oven at 80°C, and then calcine at 800°C for 2 hours to obtain Ba 0.99 Bi 0.01 TiO3@xMnO dielectric powder (x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%);

[0091] Step 6: Get the six types of Ba 0.99 Bi 0.01 TiO3@xMnO medium powders (x = 0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%) were granulated and pressed into green discs with a diameter of 10 mm and a thickness of 1.5 mm at a pressure of 8 MPa, and sintered at 1220 ° C for 2 h to obtain six kinds of Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic samples (x=0, 0.2, 0.4, 0.6, 0.8, 1.0 mol%).

[0092] See also Fig. 9 As shown, the figure shows six types of Ba #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 0.99 Bi 0.01 SEM image of TiO3@xMnO dielectric ceramic sample (SEM image is used to analyze the microscopic morphology of the ceramic surface. All dielectric ceramic samples were photographed at 13000 times. In the figure, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. In the figure, with the increase of MnO content, the grain size of the ceramic increases first and then decreases, and the grain boundaries of all dielectric ceramic samples are clear and the grain size is small. When x=0.4 mol%, it is optimal.).

[0093] See also Fig.10 As shown, the figure shows #2-1, #2-2, #2-3, #2-4, #2-5, #2-6Ba 0.99 Bi 0.01 XRD pattern of TiO3@xMnO dielectric ceramic sample (the horizontal axis in the XRD pattern is the 2θ angle, and the vertical axis is the relative intensity. In the figure, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. The figures are all pure perovskite structures, and no second phase appears. It may be that the sintering temperature is low and no manganese oxide is produced. The diffraction peak splitting of pure BBT at about 45° indicates the coexistence of tetragonal phase and cubic phase. As the MnO content increases, it gradually turns into a single peak, indicating that the content of tetragonal phase increases; the diffraction pattern shows that the manganese oxide coating can cause a slight change in the phase structure of the ceramic and promote the coexistence of multiple phases in the ceramic.).

[0094] See also Fig.11 As shown, the figure shows six types of Ba #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 0.99 Bi 0.01 Dielectric constant diagram of TiO3@xMnO dielectric ceramic samples (the horizontal axis in the dielectric constant diagram is temperature, and the vertical axis is dielectric constant. In the diagram, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. In the diagram, when x=0.8 mol%, two peaks are generated, probably one peak is the peak of the "core" BBT, and the other is the peak of the "shell" MnO, indicating that a core-shell structure is formed, and MnO is successfully coated on the BBT ceramic.).

[0095] See also Fig.12 As shown, the figure shows six types of Ba #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 0.99 Bi 0.01 Characteristic curve of dielectric loss of TiO3@xMnO dielectric ceramic samples changing with temperature (the horizontal axis of the dielectric loss graph is temperature, and the vertical axis is dielectric loss. In the figure, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. It can be seen from the figure that when x = 0.4 mol%, its dielectric loss is the lowest.).

[0096] See also Fig.13 As shown, the figure shows six types of Ba #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 0.99 Bi 0.01 Hysteresis loop diagram of TiO3@xMnO dielectric ceramic sample before breakdown (the horizontal axis of the hysteresis loop diagram is the ratio of electric field and ceramic thickness, and the vertical axis is polarization. In the figure, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are 0, 0.2 mol%, 0.4 mol%, 0.6 mol%, 0.8 mol%, and 1.0 mol% MnO dielectric ceramic samples, respectively. It can be seen from the figure that the maximum polarization value of pure BBT ceramic is the smallest and the PE loop is the smallest; after adding MnO, the maximum polarization value increases, and the energy storage density reaches the maximum value when x=0.4 mol%.).

[0097] Its main energy storage property parameters are shown in Table 2:

[0098] Table 2 shows the energy storage performance parameters of dielectric ceramic samples #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6

[0099]

[0100] In the table, #2-1, #2-2, #2-3, #2-4, #2-5, and #2-6 are dielectric ceramic samples of MnO when x=0, 0.2mol%, 0.4mol%, 0.6mol%, 0.8mol, and 1.0mol%, respectively. It can be seen from the table that as the MnO content increases, the discharge energy density of the dielectric ceramic sample increases first and then decreases. When the coating layer x=0.4mol%, the discharge energy density reaches a maximum value of 0.25J / cm 3 , and achieved a higher energy storage efficiency of 71.4%.

[0101] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0102] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material, characterized in that: Adopt Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder, the Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano powder includes a "core" part and a "shell" part, and the "core" part is made of Ba 0.99 B i0.01 TiO3, and the "shell" material is MnO.

2. The MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material according to claim 1, characterized in that: 0≤x≤1。 3. A method for preparing a MnO-coated "core-shell" structure fine-grained energy storage dielectric ceramic material as claimed in any one of claims 1 to 2, characterized in that: First, monodisperse Ba was prepared by chemical precipitation. 0.99 B i0.01 TiO3 micro-nano powder, and then prepared monodisperse MnO-coated Ba by liquid phase coating method 0.99 B i0.01 TiO3@xMnO micro-nano powder was finally sintered to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

4. The preparation method according to claim 3, characterized in that: The specific steps are as follows: Step 1, add TiCl4 solution dropwise into NaOH solution, place in a water bath at a certain temperature, and stir for a certain period of time; Step 2, preparing aqueous solutions of bismuth compound and barium compound respectively according to the stoichiometric ratio, then slowly adding the above solutions respectively and stirring evenly; Step 3: Place the obtained solution in a water bath at a certain temperature and continue stirring, then filter and dry to obtain Ba 0.99 Bi 0.01 TiO3 powder; Step 4: Ba 0.99 Bi 0.01 TiO3 powder was ultrasonically dispersed in deionized water and ethanol to obtain Ba 0.99 Bi 0.01 TiO3 suspension, then add ammonia solution and adjust the pH to alkaline environment; Step 5, prepare a manganese acetate solution using a stoichiometric ratio, then add it dropwise to the above solution while stirring to mix evenly; Step 6: The suspension is then filtered and dried to obtain micro-nano powders, and the obtained micro-nano powders are calcined in air at a certain temperature to obtain Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano dielectric powder; Step 7: Ba 0.99 Bi 0.01 TiO3@xMnO micro-nano medium powder is granulated, and after granulation, it is pressed into shape by a mold and sintered at a certain temperature to prepare Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials.

5. The method for preparing a dielectric ceramic material according to claim 4, characterized in that: Step 3 obtained Ba 0.99 Bi 0.01 TiO3 powder is a monodisperse micro-nano powder with a particle size of 50-500nm.

6. The method for preparing a dielectric ceramic material according to claim 4, characterized in that: In step 4, the pH is adjusted to 9-11.

7. The method for preparing a dielectric ceramic material according to claim 4, characterized in that: Step 6 Obtained Ba 0.99 Bi 0.01 The ceramic grains of TiO3@xMnO micro-nano dielectric powder are about 100-500nm.

8. The method for preparing a dielectric ceramic material according to claim 4, characterized in that: In step 7, the Ba 0.99 Bi 0.01 After being pressed, TiO3@xMnO micro-nano powder is sintered at 1220-1260°C for 2-6 hours to produce dielectric ceramic material.

9. The method for preparing a dielectric ceramic material according to claim 4, characterized in that: Step 7: Ba prepared 0.99 Bi 0.01 The discharge energy storage density of TiO3@xMnO dielectric ceramic materials is 0.10-0.26 J / cm 3 .

10. Ba prepared by the preparation method according to any one of claims 3 to 9 0.99 Bi 0.01 The application of TiO3@xMnO dielectric ceramic material is characterized by: The Ba 0.99 Bi 0.01 TiO3@xMnO dielectric ceramic materials are used in, but not limited to, the preparation of multilayer ceramic capacitors, positive temperature coefficient resistors, optoelectronic devices, piezoelectric sensors, and energy storage systems.

Citation Information

Patent Citations

  • Dielectric medium ceramic composition and electronic part

    CN102718478A

  • Method for doping manganese,tungsten and molybdenic dielectric ceramics powder ,and capacitor therefor

    CN1814571A

Cited By

  • High-specific-volume electrode foil and production process thereof

    CN121416327A

  • A high specific capacity electrode foil and a production process thereof

    CN121416327B