Modified barium titanate ceramic dielectric material, preparation method thereof and ceramic capacitor
By using V2O5 and/or Cr2O3 as anti-reduction agents in barium titanate materials to modify the barium titanate ceramic dielectric materials, the problems of shortened life and reduced reliability caused by the reduction of Ti4+ are solved, and low dielectric loss and excellent insulation are achieved. performance to prepare ceramic capacitors with long life and strong reliability.
Patent Information
- Application Number
- CN202410921812.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
When existing multilayer ceramic capacitors are sintered in a reducing atmosphere, Ti4+ will be reduced to Ti3+, resulting in shortened life and reduced reliability. How to effectively suppress the reduction of Ti4+ to improve the anti-reduction performance of barium titanate ceramic dielectric materials.
V2O5 and/or Cr2O3 are used as anti-reduction agents to modify the barium titanate material. Through wet ball milling, drying, granulation, tableting and high-temperature sintering, a material with low dielectric loss and excellent insulation properties is prepared. Modified barium titanate ceramic dielectric material.
It effectively inhibits the reduction of barium titanate ceramic dielectric material, improves its anti-reduction performance, and prepares long-life, highly reliable ceramic capacitors that remain stable in high-temperature applications.
Smart Images

Figure CN118754645A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dielectric materials, and in particular relates to a modified barium titanate ceramic dielectric material and a preparation method thereof, and a ceramic capacitor. Background Art
[0002] With the development of modern electronic products, multilayer ceramic capacitors (MLCC) have gradually become an indispensable part of electronic component manufacturing. Due to their many advantages such as high precision, high frequency, low power consumption, large capacity, and miniaturization, they are widely used in information technology, consumer electronics, communications, new energy, aerospace and other fields.
[0003] Due to the low cost and strong market competitiveness of materials such as nickel and copper, base metal inner electrode-multilayer ceramic capacitors (BME-MLCCs) have become the mainstream product of multilayer ceramic capacitors. When BME-MLCCs are sintered in a reducing atmosphere, Ti 4+ Will be restored to Ti 3+ , resulting in a shortened lifespan and reduced reliability of BME-MLCCs.
[0004] Therefore, how to effectively inhibit Ti 4+ Reduction to Ti 3+ , improving the anti-reduction performance of barium titanate ceramic dielectric materials, so as to obtain ceramic capacitors with long life and high reliability, is a technical problem that needs to be solved urgently. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified barium titanate ceramic dielectric material and a preparation method thereof and a ceramic capacitor. The present invention uses an anti-reducing agent including V2O5 and / or Cr2O3 to modify the barium titanate material, effectively inhibiting the reduction of the barium titanate ceramic dielectric material, improving its anti-reduction performance, and has broad development prospects. The modified barium titanate ceramic dielectric material prepared based on the preparation method has low dielectric loss and excellent insulation performance, and can be used to prepare a ceramic capacitor with long life and high reliability.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a modified barium titanate ceramic dielectric material, the preparation method comprising the following steps:
[0008] (1) mixing a barium titanate material and an anti-reducing agent, and then granulating and tableting to obtain a ceramic green body;
[0009] (2) debinding the ceramic green body, and then sintering the ceramic green body in a reducing atmosphere to obtain the modified barium titanate ceramic dielectric material;
[0010] Wherein, the anti-reducing agent includes V2O5 and / or Cr2O3.
[0011] It should be noted that the purity of the barium titanate material and the anti-reducing agent used in the present invention is above 99%.
[0012] The present invention uses an anti-reducing agent to modify the barium titanate material, effectively inhibiting the reduction of the barium titanate ceramic dielectric material, improving its anti-reduction performance, and has broad development prospects. The modified barium titanate ceramic dielectric material prepared based on the preparation method has low dielectric loss and excellent insulation performance, and can be used to prepare ceramic capacitors with long life and high reliability.
[0013] Compared with other oxides such as MgO, Bi2O3 or Nd2O3, the anti-reducing agent used in the present invention is not only a rare earth oxide, but also can be used to prepare capacitors with low temperature dependence and long life through doping, which may make the doped MLCC more stable in high-temperature applications.
[0014] Preferably, based on the molar amount of the barium titanate material in step (1), the added amount of the anti-reduction agent is 0.4-1 mol%, for example, it can be 0.4 mol%, 0.5 mol%, 0.6 mol%, 0.7 mol%, 0.8 mol%, 0.9 mol% or 1 mol%, etc., preferably 0.6-0.8 mol%.
[0015] In the present invention, if the amount of the anti-reduction agent added is too small, the dielectric loss of the ceramic dielectric material is high and the junction resistivity is low; if the amount of the anti-reduction agent added is too large, the dielectric loss of the ceramic dielectric material increases sharply and the dielectric constant is low.
[0016] Preferably, the anti-reducing agent includes V2O5 and Cr2O3, and the molar ratio of V2O5 to Cr2O3 is 1:(0.8-1.2), for example, it can be 1:0.8, 1:0.9, 1:1, 1:1.1 or 1:1.2, etc.
[0017] In the present invention, V2O5 and Cr2O3 in specific contents are used to cooperate with each other to act as anti-reducing agents, and the two produce a synergistic effect, thereby combining with oxygen vacancies to form defect dipoles, thereby restraining the movement of carriers such as free electrons and oxygen vacancy defects generated during the sintering process in a reducing atmosphere, which is beneficial to significantly reduce the dielectric loss of the modified barium titanate ceramic dielectric material and obtain excellent insulation properties.
[0018] Preferably, the mixing method in step (1) is ball milling, preferably wet ball milling.
[0019] The present invention does not limit the ball milling medium used in the wet ball milling process. For example, the ball milling medium may be a zirconia ball having a diameter of 3 mm.
[0020] Preferably, the rotation speed of the ball mill is 450-480 rpm, for example, it can be 450 rpm, 460 rpm, 470 rpm or 480 rpm.
[0021] Preferably, the ball milling time is 24-26 hours, for example, 24 hours, 25 hours or 26 hours.
[0022] Preferably, before the granulation in step (1), the mixed material is dried.
[0023] Preferably, the drying temperature is 80-100°C, for example, 80°C, 90°C or 100°C.
[0024] Preferably, the specific step of granulation in step (1) includes: adding a binder to the mixed material and granulating.
[0025] In the present invention, the function of granulation is to obtain uniformly mixed powder.
[0026] Preferably, the binder comprises polyvinyl alcohol (PVA).
[0027] Preferably, during the tableting process of step (1), the molding pressure is 350-400 MPa, for example, 350 MPa, 360 MPa, 370 MPa, 380 MPa, 390 MPa or 400 MPa.
[0028] The present invention performs tableting processing under a molding pressure of 350-400 MPa, which helps to ensure that the ceramic powder is evenly distributed during the tableting process, reduces porosity and density unevenness, and thus improves the uniformity of the sintered body.
[0029] Preferably, the specific steps of debinding in step (2) include:
[0030] The ceramic green body is subjected to primary heating and then to secondary heating.
[0031] Preferably, the temperature of the primary heating is 300-350°C, for example, it can be 300°C, 310°C, 320°C, 330°C, 340°C or 350°C, and the temperature of the secondary heating is 600-650°C, for example, it can be 600°C, 610°C, 620°C, 630°C, 640°C or 650°C.
[0032] Preferably, the heating rates of the primary heating and the secondary heating are independently 1-2°C / min, for example, 1°C / min, 1.2°C / min, 1.4°C / min, 1.6°C / min, 1.8°C / min or 2°C / min.
[0033] The purpose of heating the ceramic green body at 300-350° C. in the present invention is to remove the residual water and anhydrous ethanol in the granulation process.
[0034] Preferably, the gas in the reducing atmosphere in step (2) comprises hydrogen and an inert gas. Exemplarily, the gas in the reducing atmosphere contains 1 vol% hydrogen and 99 vol% inert gas.
[0035] Preferably, the inert gas comprises nitrogen.
[0036] In the present invention, the sintering atmosphere is limited to a reducing atmosphere in order to suppress the oxidation of base metal internal electrodes such as Ni during sintering.
[0037] Preferably, the sintering temperature in step (2) is 1200-1300°C, for example, it can be 1200°C, 1220°C, 1240°C, 1260°C, 1280°C or 1300°C.
[0038] In the present invention, if the sintering temperature is too low, sufficient densification may not be achieved, grain growth and crystal phase transformation are incomplete, and the ideal dielectric constant and capacitance value cannot be obtained; if the sintering temperature is too high, it may cause excessive grain growth, thereby increasing the dielectric loss of the capacitor, and high-temperature sintering may produce greater thermal stress, causing cracks or other defects in the MLCC.
[0039] Preferably, the sintering holding time in step (2) is 1-2 h, for example, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h.
[0040] Preferably, the preparation method comprises the following steps:
[0041] (1) wet ball milling the barium titanate material and the anti-reducing agent for 24-26 hours, drying the ball-milled powder at 80-100° C., and then sieving to obtain a powder;
[0042] Wherein, based on the molar amount of the barium titanate material, the addition amount of the anti-reduction agent is 0.4-1 mol%, the anti-reduction agent includes V2O5 and / or Cr2O3, and the rotation speed of the wet ball mill is 450-480 rpm;
[0043] (2) adding a binder to the powder for granulation, and after screening, pressing the powder into tablets under a pressure of 350-400 MPa to obtain a ceramic green body;
[0044] Wherein, based on the mass of the powder, the mass fraction of the binder is 6-10wt%;
[0045] (3) The ceramic green body is first heated to 300-350° C., kept warm for 0.5-1 h, then heated to 600-650° C., kept warm for 0.5-1 h, and debinding is completed. Then, the debinded ceramic green body is sintered in a reducing atmosphere at 1200-1300° C., kept warm for 1-2 h, and then cooled to 40-60° C. (for example, 40° C., 50° C. or 60° C., etc.) at a cooling rate of 8-10° C. / min to obtain the modified barium titanate ceramic dielectric material;
[0046] The heating rate of sintering is 3-5°C / min (for example, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min or 5°C / min, etc.).
[0047] In a second aspect, the present invention provides a modified barium titanate ceramic dielectric material, wherein the modified barium titanate ceramic dielectric material is prepared by the preparation method described in the first aspect.
[0048] Preferably, the dielectric constant of the modified barium titanate ceramic dielectric material is 1250-1850, for example, it may be 1250, 1350, 1450, 1550, 1650, 1750 or 1850, etc.
[0049] Preferably, the dielectric loss of the modified barium titanate ceramic dielectric material is ≤5.5%, for example, it may be 1%, 1.5%, 2.5%, 3.5%, 4.5% or 5.5%.
[0050] Preferably, the particle size D50 of the modified barium titanate ceramic dielectric material is 300-500 nm, for example, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm.
[0051] In a third aspect, the present invention provides a ceramic capacitor, which includes the modified barium titanate ceramic dielectric material as described in the second aspect.
[0052] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] (1) The present invention uses an anti-reduction agent including V2O5 and / or Cr2O3 to modify the barium titanate material, which effectively inhibits the reduction of the barium titanate ceramic dielectric material and improves its anti-reduction performance, and has broad development prospects.
[0055] (2) The modified barium titanate ceramic dielectric material prepared based on this preparation method has low dielectric loss and excellent insulation performance, and can be used to prepare ceramic capacitors with long life and high reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 The graph is a graph showing the dielectric constant of the modified barium titanate ceramic dielectric material prepared in Examples 1-4 of the present invention changing with temperature.
[0057] Figure 2 The graph is a graph showing the dielectric loss of the modified barium titanate ceramic dielectric material prepared in Examples 1-4 of the present invention as a function of temperature.
[0058] Figure 3 The graph is a graph showing the insulation resistivity of the modified barium titanate ceramic dielectric material prepared in Examples 1-4 of the present invention as a function of the amount of V2O5 added.
[0059] Figure 4 This is a curve diagram showing the dielectric constant of the modified barium titanate ceramic dielectric material prepared in Examples 5-8 of the present invention changing with temperature.
[0060] Figure 5 This is a curve diagram showing the dielectric loss of the modified barium titanate ceramic dielectric material prepared in Examples 5-8 of the present invention as a function of temperature.
[0061] Figure 6 This is a curve diagram showing the insulation resistivity of the modified barium titanate ceramic dielectric material prepared in Examples 5-8 of the present invention as a function of the amount of Cr2O3 added. DETAILED DESCRIPTION
[0062] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0063] Example 1
[0064] This embodiment provides a method for preparing a modified barium titanate ceramic dielectric material, the preparation method comprising the following steps:
[0065] (1) adding 23.319 g of barium titanate material and an anti-reducing agent V2O5 into a ball mill, adding zirconium oxide balls and anhydrous ethanol, and wet ball milling for 24 h, then drying the ball-milled powder at 80° C., and then sieving with a 150-mesh sieve to obtain a powder;
[0066] Wherein, based on the molar amount of the barium titanate material, the addition amount of the anti-reducing agent V2O5 is 0.4 mol%, and during the wet ball milling process, the mass ratio of the zirconium oxide balls, the ball milling material and the anhydrous ethanol is 1.5:1:1, and the ball milling speed is 480 rpm;
[0067] (2) adding 0.9 g of a binder PVA to 10 g of the powder for granulation, sieving with a 150-mesh sieve, and pressing the powder into a sheet under a pressure of 357 MPa to obtain a ceramic green body of φ8 mm×1 mm;
[0068] Wherein, based on the mass of the powder, the mass fraction of the binder PVA is 9wt%;
[0069] (3) The ceramic green body is first heated to 350°C at a heating rate of 1.5°C / min and kept at this temperature for 0.5h. Then, the temperature is heated to 650°C at a heating rate of 1.5°C / min and kept at this temperature for 0.5h to complete debinding. Then, the debinded ceramic green body is placed in a GSL-1700X dual-zone high-temperature tube furnace in a reducing atmosphere (containing 1.0vol% H2 and 99vol% N2), heated to 1250°C at a heating rate of 4°C / min for sintering, kept at this temperature for 1h, and then cooled to 50°C at a cooling rate of 9°C / min to obtain the modified barium titanate ceramic dielectric material, whose particle size D50 is 380nm.
[0070] Example 2
[0071] The difference between this embodiment and embodiment 1 is that the amount of the anti-reducing agent V2O5 added is 0.6 mol%.
[0072] The rest of the preparation methods and parameters were the same as those in Example 1.
[0073] Example 3
[0074] The difference between this embodiment and embodiment 1 is that the added amount of the anti-reducing agent V2O5 is 0.8 mol%.
[0075] The rest of the preparation methods and parameters were the same as those in Example 1.
[0076] Example 4
[0077] The difference between this embodiment and embodiment 1 is that the amount of the anti-reducing agent V2O5 added is 1 mol%.
[0078] The rest of the preparation methods and parameters were the same as those in Example 1.
[0079] Figure 1 A curve diagram showing the change of dielectric constant of the modified barium titanate ceramic dielectric material prepared in Examples 1-4 with temperature is shown. It can be seen from the figure that as the addition amount of V2O5 increases, the dielectric constant of the modified barium titanate ceramic dielectric material gradually decreases.
[0080] Figure 2 A curve chart showing the change of dielectric loss with temperature of the modified barium titanate ceramic dielectric material prepared in Examples 1-4 is shown. It can be seen from the figure that for the dielectric loss, as the V2O5 doping amount increases, its change trend is first decreasing, then suddenly increasing, and then decreasing again, and the dielectric loss shows a warping phenomenon at the high temperature end, and this phenomenon will become more obvious as the temperature increases.
[0081] Figure 3 A curve chart showing the insulation resistivity of the modified barium titanate ceramic dielectric materials prepared in Examples 1-4 as a function of the amount of V2O5 added is shown. As can be seen from the figure, the insulation resistivity gradually increases from Example 1 to Example 2, then drops suddenly in Example 3, and finally increases slightly in Example 4.
[0082] Example 5
[0083] This embodiment provides a method for preparing a modified barium titanate ceramic dielectric material, the preparation method comprising the following steps:
[0084] (1) 23.319 g of barium titanate material and anti-reducing agent Cr2O3 were added to a ball mill, and zirconium oxide balls and anhydrous ethanol were added, and wet ball milling was performed for 24 hours. The ball-milled powder was then dried at 80° C. and then sieved with a 150-mesh sieve to obtain a powder;
[0085] Wherein, based on the molar amount of the barium titanate material, the addition amount of the anti-reducing agent Cr2O3 is 0.4 mol%, and during the wet ball milling process, the mass ratio of the zirconium oxide balls, the ball milling material and the anhydrous ethanol is 1.5:1:1, and the ball milling speed is 480 rpm;
[0086] (2) adding 0.9 g of a binder PVA to 10 g of the powder for granulation, sieving with a 150-mesh sieve, and pressing the powder into a sheet under a pressure of 357 MPa to obtain a ceramic green body of φ8 mm×1 mm;
[0087] Wherein, based on the mass of the powder, the mass fraction of the binder PVA is 9wt%;
[0088] (3) The ceramic green body is first heated to 350°C at a heating rate of 1.5°C / min and kept at this temperature for 0.5h, then heated to 650°C at a heating rate of 1.5°C / min and kept at this temperature for 0.5h to complete debinding, and then the ceramic green body after debinding is placed in a GSL-1700X dual-temperature zone high-temperature tube furnace in a reducing atmosphere (containing 1.0vol% H2 and 99vol% N2), heated to 1250°C at a heating rate of 4°C / min for sintering, kept at this temperature for 1h, and then cooled to 50°C at a cooling rate of 9°C / min to obtain the modified barium titanate ceramic dielectric material, whose particle size D50 is 480nm.
[0089] Example 6
[0090] The difference between this embodiment and embodiment 5 is that the addition amount of the anti-reducing agent Cr2O3 is 0.6 mol%.
[0091] The rest of the preparation methods and parameters were the same as those in Example 5.
[0092] Example 7
[0093] The difference between this embodiment and embodiment 5 is that the added amount of the anti-reducing agent Cr2O3 is 0.8 mol%.
[0094] The rest of the preparation methods and parameters were the same as those in Example 5.
[0095] Example 8
[0096] The difference between this embodiment and embodiment 5 is that the addition amount of the anti-reducing agent Cr2O3 is 1 mol%.
[0097] The rest of the preparation methods and parameters were the same as those in Example 5.
[0098] Figure 4 A curve diagram showing the change of the dielectric constant of the modified barium titanate ceramic dielectric material prepared in Examples 5-8 with temperature is shown. It can be seen from the figure that as the addition amount of Cr2O3 increases, the dielectric constant of the modified barium titanate ceramic dielectric material gradually decreases.
[0099] Figure 5 A curve chart showing the change of dielectric loss with temperature of the modified barium titanate ceramic dielectric material prepared in Examples 5-8 is shown. It can be seen from the figure that as the addition amount of Cr2O3 increases, the change trend of the dielectric loss is first reduced and then tends to be stable.
[0100] Figure 6 A curve chart showing the change in insulation resistivity of the modified barium titanate ceramic dielectric materials prepared in Examples 5-8 as a function of the amount of Cr2O3 added is shown. It can be seen from the figure that as the amount of Cr2O3 added increases, the insulation resistivity first increases and then decreases, and the insulation resistivity of Example 6 is the largest.
[0101] Example 9
[0102] The difference between this embodiment and embodiment 1 is that the amount of the anti-reducing agent V2O5 added is 0.2 mol%.
[0103] The rest of the preparation methods and parameters were the same as those in Example 1.
[0104] Example 10
[0105] The difference between this embodiment and embodiment 1 is that the amount of the anti-reducing agent V2O5 added is 1.5 mol%.
[0106] The rest of the preparation methods and parameters were the same as those in Example 1.
[0107] Embodiment 11
[0108] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) is 1180°C.
[0109] The rest of the preparation methods and parameters were the same as those in Example 1.
[0110] Example 12
[0111] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) is 1350°C.
[0112] The rest of the preparation methods and parameters were the same as those in Example 1.
[0113] Example 13
[0114] The difference between this embodiment and embodiment 1 is that the anti-reducing agent V2O5 is replaced by a combination of V2O5 and Cr2O3, and the molar ratio of V2O5 to Cr2O3 is 1:1.
[0115] The rest of the preparation methods and parameters were the same as those in Example 1.
[0116] Embodiment 14
[0117] The difference between this embodiment and embodiment 1 is that the anti-reducing agent V2O5 is replaced by a combination of V2O5 and Cr2O3, and the molar ratio of V2O5 to Cr2O3 is 1:0.8.
[0118] The rest of the preparation methods and parameters were the same as those in Example 1.
[0119] Embodiment 15
[0120] The difference between this embodiment and embodiment 1 is that the anti-reducing agent V2O5 is replaced by a combination of V2O5 and Cr2O3, and the molar ratio of V2O5 to Cr2O3 is 1:1.2.
[0121] The rest of the preparation methods and parameters were the same as those in Example 1.
[0122] Comparative Example 1
[0123] The difference between this comparative example and Example 1 is that the anti-reducing agent V2O5 is replaced by MgO.
[0124] The rest of the preparation methods and parameters were the same as those in Example 1.
[0125] Comparative Example 2
[0126] The difference between this comparative example and Example 1 is that the reducing atmosphere in step (3) is adjusted to a nitrogen atmosphere.
[0127] The rest of the preparation methods and parameters were the same as those in Example 1.
[0128] Performance Testing
[0129] The upper and lower surfaces of the modified barium titanate ceramic dielectric material prepared in the above examples and comparative examples were polished and silver-plated, and then placed in a muffle furnace for silver infiltration treatment. After completion, the dielectric constant and dielectric loss were tested.
[0130] 1) Capacitance and losses
[0131] Test instrument: dielectric parameter tester (E4980A, Agilent, USA);
[0132] Test method: At room temperature 25°C, the driving field is adjusted to 1V / μm and the frequency is 1000Hz, and its basic electrical properties (including capacitance and dielectric loss) are measured by a dielectric parameter tester.
[0133] 2) Dielectric constant test
[0134] Test instrument: broadband dielectric tester (Alpha-A, Novocontrol GmbH, Germany);
[0135] Test method: Test capacitance and dielectric loss, then convert the dielectric constant, set the test temperature range to -60℃~200℃, the heating rate to 2℃ / min, the test frequency to 1kHz, the AC voltage to 1V, and collect data every 2℃;
[0136] The conversion formula for the dielectric constant of the wafer is as follows:
[0137]
[0138] Wherein, ε and ε0 are dielectric constant and vacuum dielectric constant, respectively, in F / m; C is capacitance, in F; d and D are thickness and diameter, respectively, in mm.
[0139] The test results are shown in Table 1.
[0140] Table 1
[0141]
[0142]
[0143] analyze:
[0144] It can be seen from the above table that the modified barium titanate ceramic dielectric material provided by the present invention has low dielectric loss and excellent insulation performance, based on which a ceramic capacitor with long life and high reliability can be prepared.
[0145] It can be seen from Examples 1 and 9-10 that if the amount of the anti-reducing agent V2O5 added is too little, the dielectric loss is high and the junction resistivity is low; if the amount of the anti-reducing agent V2O5 added is too much, the dielectric loss increases sharply and the dielectric constant is low.
[0146] It can be seen from Example 1 and Examples 11-12 that if the sintering temperature is too low, sufficient densification may not be achieved, grain growth and crystal phase transformation are incomplete, and the ideal dielectric constant and capacitance value cannot be obtained; if the sintering temperature is too high, it may cause excessive grain growth, thereby increasing the dielectric loss of the capacitor, and high-temperature sintering may produce greater thermal stress, causing cracks or other defects in the MLCC.
[0147] It can be seen from Examples 1 and 13-15 that V2O5 and Cr2O3 in a molar ratio of 1:(0.8-1.2) cooperate with each other to act as anti-reducing agents. The two can produce a synergistic effect, thereby combining with oxygen vacancies to form defect dipoles, thereby restraining the movement of carriers such as free electrons and oxygen vacancy defects generated during the sintering process in a reducing atmosphere, which is beneficial to significantly reduce the dielectric loss of the modified barium titanate ceramic dielectric material and obtain excellent insulation properties.
[0148] It can be seen from Example 1 and Comparative Example 1 that if MgO is used to modify the barium titanate material, the dielectric constant of the material is reduced and the dielectric loss is increased, making it difficult to achieve the desired technical effect of the present application.
[0149] It can be seen from Example 1 and Comparative Example 2 that if the reducing atmosphere in step (3) is adjusted to a nitrogen atmosphere, it is difficult to achieve Ti by doping an anti-reducing agent. 4+ Reduction to Ti 3+ The inhibitory effect and poor material performance.
[0150] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a modified barium titanate ceramic dielectric material, characterized in that: The preparation method comprises the following steps: (1) mixing a barium titanate material and an anti-reducing agent, and then granulating and tableting to obtain a ceramic green body; (2) debinding the ceramic green body, and then sintering the ceramic green body in a reducing atmosphere to obtain the modified barium titanate ceramic dielectric material; Wherein, the anti-reducing agent includes V2O5 and / or Cr2O3.
2. The preparation method according to claim 1, characterized in that: Based on the molar amount of the barium titanate material in step (1), the amount of the anti-reduction agent added is 0.4-1 mol%, preferably 0.6-0.8 mol%; Preferably, the anti-reduction agent comprises V2O5 and Cr2O3, and the molar ratio of V2O5 to Cr2O3 is 1:(0.8-1.2).
3. The preparation method according to claim 1 or 2, characterized in that: The mixing method in step (1) is ball milling, preferably wet ball milling; Preferably, the ball milling speed is 450-480 rpm; Preferably, the ball milling time is 24-26 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that Before the granulation in step (1), the mixed material is dried; Preferably, the drying temperature is 80-100°C; Preferably, the specific steps of granulation in step (1) include: adding a binder to the mixed material to perform granulation; Preferably, the binder comprises polyvinyl alcohol.
5. The preparation method according to any one of claims 1 to 4, characterized in that: During the tableting process of step (1), the molding pressure is 350-400 MPa.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The specific steps of debinding in step (2) include: The ceramic green body is subjected to primary heating and then to secondary heating; Preferably, the temperature of the primary heating is 300-350°C, and the temperature of the secondary heating is 600-650°C; Preferably, the gas in the reducing atmosphere in step (2) comprises hydrogen and an inert gas; Preferably, the sintering temperature in step (2) is 1200-1300° C. Preferably, the sintering holding time in step (2) is 1-2 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) wet ball milling the barium titanate material and the anti-reducing agent for 24-26 hours, drying the ball-milled powder at 80-100° C., and then sieving to obtain a powder; Wherein, based on the molar amount of the barium titanate material, the addition amount of the anti-reduction agent is 0.4-1 mol%, the anti-reduction agent includes V2O5 and / or Cr2O3, and the rotation speed of the wet ball mill is 450-480 rpm; (2) adding a binder to the powder for granulation, and after screening, pressing the powder into tablets under a pressure of 350-400 MPa to obtain a ceramic green body; Wherein, based on the mass of the powder, the mass fraction of the binder is 6-10wt%; (3) first heating the ceramic green body to 300-350° C., keeping the temperature for 0.5-1 h, then heating to 600-650° C., keeping the temperature for 0.5-1 h, completing debinding, then sintering the debinded ceramic green body in a reducing atmosphere at 1200-1300° C., keeping the temperature for 1-2 h, and then cooling to 40-60° C. at a cooling rate of 8-10° C. / min to obtain the modified barium titanate ceramic dielectric material; The sintering heating rate is 3-5°C / min.
8. A modified barium titanate ceramic dielectric material, characterized in that: The modified barium titanate ceramic dielectric material is prepared by the preparation method according to any one of claims 1 to 7.
9. The modified barium titanate ceramic dielectric material according to claim 8, characterized in that: The dielectric constant of the modified barium titanate ceramic dielectric material is 1250-1850; Preferably, the dielectric loss of the modified barium titanate ceramic dielectric material is ≤5.5%; Preferably, the particle size D50 of the modified barium titanate ceramic dielectric material is 300-500 nm.
10. A ceramic capacitor, characterized in that: The ceramic capacitor comprises the modified barium titanate ceramic dielectric material as claimed in claim 8 or 9.
Citation Information
Patent Citations
Anti-reducing low-loss barium titanate-based dielectric material
CN109020537A
Anti-reduction BME ceramic dielectric capacitor and ceramic material for capacitor
CN112645708A
Co-doped barium titanate ceramic dielectric material as well as preparation method and application thereof
CN114014649A
Dielectric composition and ceramic capacitor using same
JP2000264729A
Dielectric ceramic composition
JP2002037663A