Barium titanate-based leadless piezoelectric ceramic and preparation method thereof
Through the chemical structure and preparation method of barium titanate-based lead-free piezoelectric ceramics, combined with the doping of LiNbO3, BiZrO3 and CuO, the environmental hazards and performance deficiencies of lead-containing ceramics are solved, and high voltage electrical performance and high Curie temperature are achieved Lead-free piezoelectric ceramic materials have practical industrial application value.
Patent Information
- Application Number
- CN202411013472.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lead-containing piezoelectric ceramic materials contain toxic lead elements, which cause environmental and human hazards, and the piezoelectric constant and Curie temperature of barium titanate piezoelectric ceramics that have not been doped and modified are insufficient, limiting their use. application.
Using the chemical structural formula of barium titanate-based lead-free piezoelectric ceramics (Ba1-xLnx)(Ti1-yMny)O3-αwt%LiNbO3-βwt%BiZrO3-γwt%CuO, through A-site and B-site double doping, combined with LiNbO3, The addition of BiZrO3 and CuO improves the piezoelectric properties, and the sintering process is carried out through a specific preparation method.
The piezoelectric properties and Curie temperature of barium titanate-based lead-free piezoelectric ceramics are significantly improved, forming a new lead-free piezoelectric ceramic system with excellent thermal stability, which has practical industrial application significance.
Smart Images

Figure CN118754647A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of piezoelectric ceramic materials, in particular to a barium titanate-based lead-free piezoelectric ceramic and a preparation method thereof. Background Art
[0002] Piezoelectric ceramics have been widely used in sensors, transducers, drivers and micro-displacement generators due to their important functional properties. In the past few decades, the dominant piezoelectric ceramics are mainly lead-containing ceramics, such as PZT, PMN, PZN, etc. These ceramics have excellent piezoelectric properties, but they all contain a large amount of toxic lead elements, which will cause great harm to the environment and human body. As people pay more attention to environmental protection issues, finding new lead-free piezoelectric ceramics to replace lead-containing piezoelectric ceramics has become a hot spot in material research.
[0003] Barium titanate has been widely studied as a ferroelectric solid solution with a perovskite structure, but the piezoelectric constant d of undoped and unmodified barium titanate piezoelectric ceramics is 33 It is only about 190 pC / N, and the low Curie temperature also seriously limits its practical application. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a barium titanate-based lead-free piezoelectric ceramic and a preparation method thereof.
[0005] The technical solutions adopted are as follows: A barium titanate-based lead-free piezoelectric ceramic, the chemical structure of which is as follows: (Ba 1-x Ln x )(Ti 1-y Mn y )O3-αwt%LiNbO3-βwt%BiZrO3-γwt%CuO Among them, Ln is a lanthanide element; 0<x≤0.5, 0<y≤0.5; 0<α≤10, 0<β≤10, 0<γ≤5.
[0006] Furthermore, Ln is any one or more of La, Nd, Dy, Yb, and Lu.
[0007] Furthermore, 0.01≤x≤0.1, 0.1≤y≤0.3.
[0008] Further, x=0.05, y=0.2.
[0009] Furthermore, 1≤α≤5, 1≤β≤5, 0.1≤γ≤1.
[0010] Furthermore, α=4, β=1, and γ=0.5.
[0011] The present invention also provides a method for preparing a barium titanate-based lead-free piezoelectric ceramic: BaCO3, Ln oxide, TiO2, and MnO2 are mixed and ball-milled, and then pre-fired once. Then, they are mixed with LiNbO3, BiZrO3, and CuO, and then ball-milled again and pre-fired twice to obtain a mixed powder. The mixed powder is granulated, sieved, pressed, debinded, and sintered at 1350-1550°C for 2-4h.
[0012] Furthermore, the temperature of the first pre-firing is 1000-1050° C., the time of the first pre-firing is 2-4 hours, the temperature of the second pre-firing is 1150-1200° C., and the time of the second pre-firing is 2-4 hours.
[0013] Furthermore, the pressure during pressing is 100-200 MPa.
[0014] Furthermore, the debinding temperature is 600-800°C, and the debinding time is 1-3h.
[0015] Beneficial effects of the present invention: The present invention provides a barium titanate-based lead-free piezoelectric ceramic. By doping the A and B positions of BaTiO3, a donor-acceptor defect complex can be formed to improve the piezoelectric properties of barium titanate. LiNbO3 has an extremely high Curie temperature. As a distorted perovskite structure compound, it can significantly increase the Curie temperature of piezoelectric ceramic materials after being added, thereby obtaining a new lead-free piezoelectric ceramic system with excellent thermal stability. 3+ It has a non-inert gas outer electron structure, and Bi 3+ and Zr 3+ They can all be dissolved in the perovskite lattice, and can play a doping and modification role in the piezoelectric properties of the piezoelectric ceramic system. After addition, the piezoelectric properties of the lead-free piezoelectric ceramic system are greatly improved. The barium titanate-based lead-free piezoelectric ceramics prepared by the present invention have excellent piezoelectric properties and a high Curie temperature, and have practical industrial application significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a cross-sectional scanning electron microscope image of the barium titanate-based lead-free piezoelectric ceramic prepared in Example 1. It can be observed that the internal microstructure is uniform, without obvious pores and precipitates, and the structure is relatively dense. DETAILED DESCRIPTION
[0017] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters. Example 1
[0018] A barium titanate-based lead-free piezoelectric ceramic, the chemical structure of which is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and then mixed with LiNbO3, BiZrO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h. Example 2
[0019] A barium titanate-based lead-free piezoelectric ceramic, the chemical structure of which is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 4h. After the pre-fired, it is restored to room temperature and mixed with LiNbO3, BiZrO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, adopt forward and reverse alternating ball milling, the interval time is 1h, the total ball milling time is 10h, the mixed material obtained by ball milling is dried and then pre-fired for the second time at 1200℃, the secondary pre-fired time is 4h, 8wt% PVA solution is added to the mixed powder after the secondary pre-fired to make granules, and after passing through an 80-mesh sieve, it is pressed into a green body at 100MPa, and the green body is placed in a muffle furnace, first heated to 800℃ at a rate of 1℃ / min, kept for debinding for 3h, and then heated to 1550℃ at a rate of 5℃ / min and sintered for 4h. Example 3
[0020] A barium titanate-based lead-free piezoelectric ceramic, the chemical structure of which is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1000℃ for 2h. After the pre-fired, it is restored to room temperature and then mixed with LiNbO3, BiZrO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, using forward and reverse alternating ball milling with an interval of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling is dried, it is pre-fired for the second time at 1150℃ for 2h. 8wt% PVA solution is added to the mixed powder after the second pre-fired to make granules. After passing through an 80-mesh sieve, it is pressed into a green body at 100MPa. The green body is placed in a muffle furnace, first heated to 600℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1400℃ at a rate of 5℃ / min and sintered for 2h. Example 4
[0021] The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: (Ba 0.95 La 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, La2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and then mixed with LiNbO3, BiZrO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0022] Comparative Example 1: The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3 Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and poured into the ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0023] Comparative Example 2: The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: BaTiO3-4wt%LiNbO3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3 and TiO2 are poured into a ball mill for ball milling and mixing, wherein the ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the forward and reverse alternating ball mill is adopted, the interval time is 1h, and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and then mixed with LiNbO3, BiZrO3, and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0024] Comparative Example 3: The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-1wt%BiZrO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and then mixed with BiZrO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill, the ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0025] Comparative Example 4: The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-0.5wt%CuO Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, the ball milling speed is 300 r / min, and the forward and reverse alternating ball mill is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and mixed with LiNbO3 and CuO, and poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar, the ball milling balls are zirconia balls, the ball milling medium is anhydrous ethanol, the ball-to-material ratio is 5:1, and the ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0026] Comparative Example 5: The embodiment is basically the same as the embodiment 1, except that the embodiment provides a barium titanate-based lead-free piezoelectric ceramic, and the chemical structure thereof is as follows: (Ba 0.95 Dy 0.05 )(Ti 0.8 Mn 0.2 )O3-4wt%LiNbO3-1wt%BiZrO3 Preparation method of the above-mentioned barium titanate-based lead-free piezoelectric ceramic: BaCO3, Dy2O3, TiO2 and MnO2 are poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar. The ball milling balls are zirconia balls. The ball milling medium is anhydrous ethanol. The ball-to-material ratio is 5:1. The ball milling speed is 300 r / min. The forward and reverse alternating ball milling is adopted. The interval time is 1h and the total ball milling time is 10h. After the mixed material obtained by ball milling is dried, it is pre-fired at 1050℃ for 3h. After the pre-fired, it is restored to room temperature and mixed with LiNbO3 and BiZrO3. It is poured into a ball mill for ball milling and mixing. The ball mill is a micro planetary ball mill. The ball mill adopts a nylon jar. The ball milling balls are zirconia balls. The ball milling medium is anhydrous ethanol. The ball-to-material ratio is 5:1. The ball milling speed is 300 r / min, and adopted positive and reverse alternating ball milling with an interval time of 1h and a total ball milling time of 10h. After the mixed material obtained by ball milling was dried, it was pre-fired for the second time at 1180℃ for 3h. 8wt% PVA solution was added to the mixed powder after the secondary pre-fired to make granules. After passing through an 80-mesh sieve, it was pressed into a green body at 100MPa. The green body was placed in a muffle furnace, first heated to 750℃ at a rate of 1℃ / min, kept for debinding for 2h, and then heated to 1450℃ at a rate of 5℃ / min and sintered for 3h.
[0027] Performance Test: The surfaces of the barium titanate-based lead-free piezoelectric ceramics prepared in Examples 1-4 and Comparative Examples 1-5 were polished, coated with silver paste on both sides, kept at 750°C for 10 min, and finally polarized at a DC voltage of 4 kV / mm for 20 min in silicone oil at 120°C and placed for 24 h to test their electrical properties as samples.
[0028] The room temperature piezoelectric constant of the sample was measured using a ZJ-3AN quasi-static piezoelectric constant tester. The electromechanical coupling coefficient kp, mechanical quality factor Qm and dielectric loss tanδ (25°C, 1V, 1kHz) of the samples were measured and analyzed using a precision impedance analyzer (Agilent HP4294A). According to GBT3389.3 "Test Methods for Performance of Piezoelectric Ceramic Materials Curie Temperature T c Test》Test and calculate the Curie temperature T of the sample c ; The test results are shown in Table 1 below: Table 1: d33 (pC / N) kp Q tanδ Tc(℃) Example 1 790 0.63 440 0.43% 243 Example 2 773 0.62 431 0.47% 237 Example 3 754 0.59 425 0.48% 234 Example 4 739 0.58 401 0.53% 230 Comparative Example 1 316 0.45 240 1.8% 135 Comparative Example 2 608 0.52 327 1.1% 220 Comparative Example 3 624 0.55 342 0.96% 183 Comparative Example 4 652 0.56 361 0.78% 197 Comparative Example 5 689 0.58 388 0.61% 226 It can be seen from Table 1 above that the barium titanate-based lead-free piezoelectric ceramics prepared in the present invention have excellent piezoelectric properties and a relatively high Curie temperature, and have practical industrial application significance.
[0029] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A barium titanate-based lead-free piezoelectric ceramic, characterized in that: Its chemical structure is as follows: (Off 1-x Ln x )(It 1-y Mn y )O3-αwt%LiNbO3-βwt%BiZrO3-γwt%CuO Among them, Ln is a lanthanide element; 0<x≤0.5, 0<y≤0.5; 0<α≤10, 0<β≤10, 0<γ≤5.
2. The barium titanate-based lead-free piezoelectric ceramic according to claim 1, characterized in that: Ln is any one or more of La, Nd, Dy, Yb, and Lu.
3. The barium titanate-based lead-free piezoelectric ceramic according to claim 1, characterized in that: 0.01≤x≤0.1, 0.1≤y≤0.
3.
4. The barium titanate-based lead-free piezoelectric ceramic according to claim 1, characterized in that: x=0.05,y=0.
2.
5. The barium titanate-based lead-free piezoelectric ceramic according to claim 1, characterized in that: 1≤α≤5, 1≤β≤5, 0.1≤γ≤1.
6. The barium titanate-based lead-free piezoelectric ceramic according to claim 1, characterized in that: α=4, β=1, γ=0.
5.
7. A method for preparing a barium titanate-based lead-free piezoelectric ceramic according to any one of claims 1 to 6, characterized in that: BaCO3, Ln oxide, TiO2, and MnO2 are mixed and ball-milled, and then pre-fired once. Then, they are mixed with LiNbO3, BiZrO3, and CuO, and then ball-milled again and pre-fired twice to obtain a mixed powder. The mixed powder is granulated, sieved, pressed, debinded, and sintered at 1350-1550°C for 2-4h.
8. The method for preparing the barium titanate-based lead-free piezoelectric ceramic according to claim 7, characterized in that: The temperature of the first pre-burning is 1000-1050°C, the time of the first pre-burning is 2-4h, the temperature of the second pre-burning is 1150-1200°C, and the time of the second pre-burning is 2-4h.
9. The method for preparing the barium titanate-based lead-free piezoelectric ceramic according to claim 7, characterized in that: The pressure during pressing is 100-200MPa.
10. The method for preparing the barium titanate-based lead-free piezoelectric ceramic according to claim 7, characterized in that: The debinding temperature is 600-800℃ and the debinding time is 1-3h.
Citation Information
Cited By
Barium titanate electronic ceramic and preparation method thereof
CN118978398A