Compact nano transition metal carbide high-entropy ceramic and preparation method thereof

Through the sol-gel method and discharge plasma sintering process, the problem of large particle size and difficulty in sintering of high-entropy carbide ceramics is solved, and the preparation of high-entropy carbide ceramics with high density and nano-scale grain size is achieved, which satisfies the requirements of high-entropy carbide ceramics. Density and grain size requirements for carbide ceramics.

CN118754669AActive Publication Date: 2024-10-11ZHENGZHOU UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410976762.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-21
Publication Date
2024-10-11
Estimated Expiration
2044-07-21

AI Technical Summary

Technical Problem

The particle size of high-entropy carbide ceramics prepared in the prior art is greater than 100 nm, which makes sintering difficult, and the sintering of nano-scale high-entropy carbide ceramics has not yet been realized.

Method used

The high-entropy carbide precursor is prepared using the sol-gel method, and the ceramic grain size and composition uniformity are controlled through high-temperature cracking and discharge plasma sintering processes to achieve the preparation of dense nano-transition metal carbide high-entropy ceramics.

Benefits of technology

The density of high-entropy carbide ceramics is greater than 95%, and the grain size is 70-80nm, which meets the requirements of density, purity and grain size, and simplifies the preparation process and shortens the production cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754669A_ABST
    Figure CN118754669A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramics, and discloses a compact nano transition metal carbide high-entropy ceramic and a preparation method thereof.The preparation method comprises the steps that firstly, transition metal salt and a carbon source are mixed and stirred in an organic solvent at the temperature of 50-70 DEG C, and high-entropy carbide precursor wet gel is obtained; and drying the high-entropy carbide precursor wet gel to obtain high-entropy carbide precursor xerogel, grinding the high-entropy carbide precursor xerogel into powder, carrying out thermal insulation cracking in a protective atmosphere, and carrying out spark plasma sintering on the cracked powder at 1900-2000 DEG C to obtain the compact nano transition metal carbide high-entropy ceramic. The density of the prepared high-entropy carbide ceramic is larger than 95%, components are uniform, the grain size ranges from 70 nm to 80 nm, and the requirements of the high-entropy carbide ceramic for density, purity and grain size can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramics, and relates to the preparation of nanometer carbide ceramics, and in particular to a dense nanometer transition metal carbide high entropy ceramic and a preparation method thereof. Background Art

[0002] Single-component transition metal (IVB–VB group) carbide ceramics are a type of ceramic material with a melting point greater than 3000°C, which can be used for a long time in high temperature environments, and has excellent ablation resistance, high temperature mechanical properties and thermal shock resistance. They are widely used in the aerospace field, such as hypersonic vehicles, rocket propulsion, and reentry vehicles. In recent years, the method of improving the intrinsic properties of materials through high entropy has attracted widespread attention. High entropy carbide ceramics are solid solutions composed of more than five transition metal carbides of groups IVB, VB and VIB, with strong covalent bonds, chemical disorder and four major effects (high entropy effect, hysteresis diffusion effect, lattice distortion effect and cocktail effect). Compared with single-component carbide ceramics, high-entropy carbide ceramics have many excellent properties, including high hardness, high elastic modulus, excellent mechanical properties, good oxidation resistance, good thermal stability and adjustable thermal conductivity. In addition, high-entropy materials have huge space for composition design and performance regulation, which brings unlimited challenges and possibilities to the development of new materials and can meet the needs of extreme (high temperature, high pressure, corrosion, radiation, stress) environments such as aviation, aerospace, navigation, nuclear energy, etc.

[0003] Patent application CN 110104648 A discloses a high entropy carbide nanopowder and a preparation method thereof. The nanopowder is prepared by a sol-gel reaction between a transition metal salt and an organic carbon source. The particle size of the ceramic nanopowder is 100-200nm. Patent application CN 115772034 A discloses a high entropy carbide ceramic precursor, a high entropy carbide ceramic and a preparation method. The high entropy carbide ceramic precursor obtained by the method is in a liquid state and is easy to store, but the grain size of the ceramic finally prepared is distributed between 100-200nm. Patent application CN 116514553 A discloses a composite carbide ceramic powder material and its preparation method and application. The components of the high entropy carbide powder prepared by the sol-gel method are uniformly distributed, and the obtained high entropy powder is submicron (-350nm). In summary, the particle size of the high entropy carbide powders reported so far is greater than 100 nm. Due to the presence of a large number of covalent bonds in carbide ceramics and high entropy carbides, they are difficult to sinter, and the sintering of nanoscale high entropy carbide ceramics is still a blank. Summary of the invention

[0004] The present invention aims to solve the above problems in the prior art and provide a dense nano-transition metal carbide high-entropy ceramic and a preparation method thereof, which can precisely control the ceramic grain size while regulating the uniformity of the high-entropy ceramic composition.

[0005] Sol-gel method is different from the traditional powder metallurgy preparation process. It is a method to obtain nano ceramic powder by high temperature cracking and sintering of carbide high entropy precursor. It can achieve uniform molecular size composition, obtain nano-sized powder, and reduce the synthesis temperature. Spark plasma sintering (SPS) is a rapid sintering process for preparing bulk materials through field-assisted sintering. While controlling the ceramic grain size, it also promotes the solid solution of high entropy ceramics and quickly completes the densification of ceramics.

[0006] In view of this, the present application proposes a method for preparing dense nano transition metal carbide high entropy ceramics using a sol-gel precursor, comprising the following steps:

[0007] (1) mixing a transition metal salt and a carbon source in an organic solvent at 50-70° C. and stirring to obtain a high entropy carbide precursor wet gel; the transition metal salt and the carbon source are measured according to a molar ratio of transition metal to carbon of (1.2-1):(1-5);

[0008] (2) The high entropy carbide precursor wet gel is dried to obtain a high entropy carbide precursor dry gel;

[0009] (3) grinding the obtained high entropy carbide precursor dry gel into powder, and then pyrolyzing it under a protective atmosphere;

[0010] (4) The pyrolyzed powder is spark plasma sintered at 1900-2000°C to obtain dense nano-transition metal carbide high entropy ceramics.

[0011] In the above step (1), the transition metal salt includes at least one transition metal chloride; the transition metal (IVB-VB group) is selected from Ti, Nb, Ta, Cr, Mo, Zr, W, V or Hf; in the sol-gel process for preparing nanopowders, in a preferred embodiment, the transition metal salt includes three or more transition metal chlorides, and the carbon source is at least one of furfuryl alcohol, starch, glucose, etc. The organic solvent is ethanol. The transition metal salt and the carbon source are mixed and stirred in an organic solvent for 1-2 hours to obtain a high entropy carbide precursor wet gel.

[0012] In the above step (2), the high entropy carbide precursor wet gel is dried at 100-170° C. to obtain a high entropy carbide precursor dry gel, and the heat preservation time is 12-18 hours.

[0013] In the above step (3), the high entropy carbide precursor dry gel used is ground to a powder particle size range of 200-400 mesh. The pyrolysis temperature of the high entropy carbide precursor dry gel can be determined according to infrared spectroscopy and thermogravimetric analysis; it has been found that the pyrolysis temperature of the high entropy carbide precursor dry gel is 1000-1600°C, and the pyrolysis temperature insulation time is 1-2h; the pyrolysis temperature program is: heating or cooling at 3-5°C / min, divided into 2-3 gradient heating, each temperature section is kept warm for 30-90min, when the temperature is raised to 1000-1600°C, continue to keep warm for 1-2h, and then cool to room temperature. The protective atmosphere used is argon or nitrogen. The pyrolysis yield is 30-55%.

[0014] In the above step (4), the cracked powder is first ball milled and then spark plasma sintered; the ball milling speed is 80-120rpm and the time is 10-14h. Spark plasma sintering is carried out at ≤5×10 -2 Pa vacuum, the heating or cooling rate is 50-100℃ / min, divided into 2-3 gradient heating or cooling, and the temperature is kept for 10-25min after heating to the set maximum temperature. The spark plasma sintering pressure is 40-65MPa.

[0015] The dense nano transition metal carbide high entropy ceramic prepared by the method has a grain size of 70-80nm, a porosity of 0-5% (excluding the end value 0), and a density greater than 95%.

[0016] Compared with the prior art, the transition metal carbide high entropy ceramic and the preparation method thereof provided by the present invention have the following beneficial effects:

[0017] (1) The present invention adopts a sol-gel precursor method to prepare high entropy carbide ceramics. The carbide precursor is prepared by the sol-gel method, and high-temperature pyrolysis is performed to cause a carbon thermal reduction reaction to obtain nano-scale high entropy carbide; therefore, adjusting the dry gel pyrolysis process can improve the density, composition control and uniformity of the high entropy carbide ceramics.

[0018] (2) The present invention adopts spark plasma sintering, which has the advantages of high heating rate, low sintering temperature, short sintering time, etc., and can make high entropy carbide ceramics dense while inhibiting the growth of ceramic grains and sintering quickly.

[0019] (3) The preparation method provided by the present invention enables the prepared high entropy carbide ceramics to have a density greater than 95% (can reach 95.09%-99.86% in the embodiment), uniform composition, and a grain size of 70-80nm, which can meet the requirements of high entropy carbide ceramics for density, purity and grain size.

[0020] (4) The method for preparing transition metal carbide high entropy ceramics provided by the present invention is simple to operate, has a short production cycle, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a process flow chart of the transition metal carbide high entropy ceramic of the present invention;

[0022] Figure 2 Optimize the high-temperature cracking curve for the tubular furnace; (a) corresponds to the 1000℃ cracking curve, and (b) corresponds to the 1600℃ cracking curve.

[0023] Figure 3 is the SPS sintering system curve;

[0024] Figure 4 are the results of pyrolysis analysis; wherein (a) is the thermogravimetric analysis curve of the sol-gel precursor xerogel prepared in Example 5, and (b) is the infrared spectrum of the pyrolysis products prepared in Example 4, Example 5, and Example 6;

[0025] Figure 5 XRD patterns of dense nano transition metal carbide high entropy ceramics prepared in Examples 2 to 5;

[0026] Figure 6 This is the high-resolution TEM and elemental energy spectrum analysis of Example 4. DETAILED DESCRIPTION

[0027] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0028] The preparation method of the transition metal carbide high entropy ceramics used in the following embodiments of the present invention is as follows: Figure 1 As shown, the following steps are included:

[0029] (1) mixing transition metal chloride powder and a carbon source in ethanol at 50-70° C. and stirring to obtain a high entropy carbide precursor wet gel; the transition metal salt and the carbon source are measured according to a molar ratio of transition metal to carbon of (1.2-1):(1-5); and the stirring time is 1-2 h;

[0030] (2) The high entropy carbide precursor wet gel is dried to obtain a high entropy carbide precursor dry gel; the drying temperature is 100-170° C., and the insulation time is 12-18 h;

[0031] (3) The obtained high entropy carbide precursor dry gel is ground into powder (the final particle size range is 200-400 mesh), and then pyrolyzed under a protective atmosphere; the pyrolysis temperature is 1000-1600°C, the pyrolysis temperature holding time is 1-2h, and the protective atmosphere used is argon or nitrogen; the pyrolysis temperature program is: the pyrolysis temperature program is: heating or cooling at 3-5°C / min, divided into 2-3 gradient heating, each temperature section is kept for 30-90min, when the temperature is raised to 1000-1600°C, continue to keep warm for 1-2h, and then cool to room temperature;

[0032] (4) The pyrolyzed powder is subjected to spark plasma sintering at 1900-2000°C to obtain transition metal carbide high entropy ceramics; the specific operation is: the pyrolyzed powder is first ball milled and then spark plasma sintered; the ball milling speed is 80-120 rpm and the time is 10-14 h; the spark plasma sintering is carried out at ≤5×10 -2 Pa vacuum, the heating or cooling rate is 50-100℃ / min, divided into 2-3 gradient heating or cooling, and the temperature is kept for 10-25min after heating to the set maximum temperature. The spark plasma sintering pressure is 40-65MPa.

[0033] The high entropy carbide precursor wet gel obtained in step (1) or the high entropy carbide precursor dry gel obtained in step (2) can be subjected to thermogravimetry (TG) / differential scanning calorimetry (DSC) and infrared testing (FTIR) to optimize the pyrolysis temperature.

[0034] Example 1

[0035] The transition metal salt used in this example is TiCl 4 The carbon source is furfuryl alcohol (C 5 H 6 O 2 ), TiCl 4 The molar ratio of furfuryl alcohol is 6:1.

[0036] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0037] (1) 151.38 g TiCl 4 Add to 70g of ethanol solution and stir evenly; then add 13g of furfuryl alcohol to the resulting mixture and stir at 60°C for 1h to obtain a high entropy carbide precursor wet gel;

[0038] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0039] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tube furnace and pyrolyzed at 1000°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as shown in FIG. Figure 2 (a) shown.

[0040] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale TiC ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10 minutes; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as shown in Figure 2. Figure 3 shown.

[0041] Example 2

[0042] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 The carbon source is furfuryl alcohol (C 5 H 6 O 2 ), TiCl 4 、NbCl 5 、TaCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 6:1.

[0043] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0044] (1) 36.04 g TiCl 4 、51.34gNbCl 5 、68.05gTaCl 5 Add to 70g of ethanol solution and stir evenly; then add 9.34g of furfuryl alcohol to the resulting mixture and stir at 60°C for 1h to obtain a high entropy carbide precursor wet gel;

[0045] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0046] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tube furnace and pyrolyzed at 1000°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as shown in FIG. Figure 2 (a)

[0047] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTa)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as Figure 3 shown.

[0048] Example 3

[0049] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 The carbon source is furfuryl alcohol (C 5 H 6 O 2 ), TiCl 4 、NbCl 5 、TaCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 6:1.

[0050] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0051] (1) 36.04 g TiCl 4 、51.34gNbCl 5 、68.05gTaCl 5Add to 70g of ethanol solution and stir evenly; then add 9.34g of furfuryl alcohol to the resulting mixture and stir at 60°C for 1h to obtain a high entropy carbide precursor wet gel;

[0052] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0053] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tubular furnace, and pyrolyzed at 1600°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, then the temperature was increased to 1600°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as Figure 2 (b)

[0054] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTa)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as Figure 3 shown.

[0055] Example 4

[0056] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 , carbon source is furfuryl alcohol, TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 6:1.

[0057] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0058] (1) 22.76 g TiCl 4 、32.42gNbCl 5 、42.98gTaCl 5 、19gCrCl 3 、32.78gMoCl 5 Add to 70g ethanol solution and stir evenly; then add 9.72g furfuryl alcohol (C 5 H 6 O 2 ), and stirred at 60°C for 1 h to obtain a high entropy carbide precursor wet gel;

[0059] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0060] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tube furnace and pyrolyzed at 1000°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as shown in FIG. Figure 2 (a)

[0061] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTaCrMo)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as shown in Figure 2. Figure 3 shown.

[0062] Example 5

[0063] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 CrCl3 、MoCl 5 , carbon source is furfuryl alcohol, TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 1:1.

[0064] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0065] (1) 3.6 g TiCl 4 、5.13gNbCl 5 、6.8gTaCl 5 、3gCrCl 3 、5.19gMoCl 5 Add to 70g ethanol solution and stir evenly; then add 9.52g furfuryl alcohol (C 5 H 6 O 2 ), and stirred at 60°C for 1 h to obtain a high entropy carbide precursor wet gel;

[0066] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0067] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tubular furnace, and pyrolyzed at 1600°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, then the temperature was increased to 1600°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as Figure 2 (b)

[0068] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTaCrMo)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as shown in Figure 2. Figure 3 shown.

[0069] Example 6

[0070] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 , carbon source is furfuryl alcohol, TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 1:1.

[0071] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0072] (1) 5.12 g TiCl 4 、7.29g NbCl 5 、9.67g TaCl 5 、4.28g CrCl 3 、7.38g MoCl 5 Add to 70g ethanol solution and stir evenly; then add 13.32g furfuryl alcohol (C 5 H 6 O 2 ), and stirred at 60°C for 1 h to obtain a high entropy carbide precursor wet gel;

[0073] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 120° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0074] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tubular furnace, and pyrolyzed at 1500°C for 1 hour under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 minutes, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 minutes, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 minutes, then the temperature was increased to 1500°C at 5°C / min and kept at this temperature for 60 minutes, and then the temperature was decreased to room temperature at 5°C / min;

[0075] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 90 rpm for 12 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree, pressure 40MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTaCrMo)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as shown in Figure 2. Figure 3 shown.

[0076] Example 7

[0077] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 , carbon source is glucose, TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 The molar ratio of is 1:1:1:1:1; the molar ratio of all transition metal chlorides to glucose is 6:1.

[0078] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0079] (1) 13.66 g TiCl 4 、19.45gNbCl 5 、25.79gTaCl 5 、11.4gCrCl 3 、19.67gMoCl 5Add to 70g ethanol solution and stir evenly; then add 11g glucose (C 6 H 12 O 6 ), and stirred at 50°C for 2 h to obtain a high entropy carbide precursor wet gel;

[0080] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 100° C. for 18 h to obtain a high entropy carbide precursor dry gel;

[0081] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tubular furnace, and pyrolyzed at 1000°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was: first, the temperature was increased to 300°C at 3°C / min, and the temperature was kept for 60 min, then the temperature was increased to 600°C at 5°C / min, and the temperature was kept for 60 min, then the temperature was increased to 1000°C at 5°C / min, and the temperature was kept for 60 min, and then the temperature was decreased to room temperature at 5°C / min;

[0082] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 80 rpm for 14 h; then placed in a mold and sintered in a spark plasma sintering furnace at ≤5×10 -2 Pa vacuum degree and pressure of 40MPa, spark plasma sintering was carried out according to the heating program and the cooling program to obtain nanoscale (TiNbTaCrMo)C ceramics; the heating program was: from room temperature to 1500℃ at 100℃ / min, then to 1900℃ at 80℃ / min, and sintered for 25min; the cooling program was: from 80℃ / min to 1500℃, then to room temperature at 100℃ / min.

[0083] Example 8

[0084] The transition metal salt used in this example is TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 , carbon source is furfuryl alcohol, TiCl 4 、NbCl 5 、TaCl 5 CrCl 3 、MoCl 5 The molar ratio of all transition metal chlorides to furfuryl alcohol is 1:1. `

[0085] The preparation method of the transition metal carbide high entropy ceramic provided in this embodiment comprises the following steps:

[0086] (1) 3.6 g TiCl4 、5.13gNbCl 5 、6.8gTaCl 5 、3gCrCl 3 、5.19gMoCl 5 Add to 70g of ethanol solution and stir evenly; then add 9.52g of furfuryl alcohol to the resulting mixture and stir at 70°C for 1h to obtain a high entropy carbide precursor wet gel;

[0087] (2) placing the obtained high entropy carbide precursor wet gel in an oven and drying it at 170° C. for 12 h to obtain a high entropy carbide precursor dry gel;

[0088] (3) The obtained high entropy carbide precursor dry gel was ground into a powder with a particle size range of 200-400 mesh, and then placed in a tubular furnace, and pyrolyzed at 1600°C for 1 h under an argon protective atmosphere; the pyrolysis temperature program was as follows: first, the temperature was increased to 350°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 600°C at 3°C / min and kept at this temperature for 60 min, then the temperature was increased to 1000°C at 5°C / min and kept at this temperature for 60 min, then the temperature was increased to 1600°C at 5°C / min and kept at this temperature for 60 min, and then the temperature was decreased to room temperature at 5°C / min, as Figure 2 (b)

[0089] (4) The pyrolyzed powder was placed in a ball mill and milled at a speed of 120 rpm for 10 h. Then, the powder was placed in a mold and sintered in a spark plasma sintering furnace at a temperature of ≤5×10 -2 Pa vacuum degree, pressure 65MPa, spark plasma sintering was carried out according to the heating program and cooling program to obtain nano-scale (TiNbTaCrMo)C ceramics; the heating program was: from room temperature to 1500°C at 100°C / min, then to 1900°C at 80°C / min, then to 2000°C at 50°C / min, and sintered for 10min; the cooling program was: from 2000°C to 1900°C at 50°C / min, then to 1500°C at 80°C / min, and then to room temperature at 100°C / min, as shown in Figure 2. Figure 3 shown.

[0090] Cracking process research

[0091] The high entropy carbide precursor xerogel prepared in step (2) of Example 5 was subjected to thermogravimetric (TG) analysis and differential scanning calorimetry (DSC) analysis. The results are as follows: Figure 4 The pyrolysis products prepared in step (3) of Example 4, Example 5 and Example 6 were subjected to infrared testing and analysis, and the results were as follows: Figure 4 (b) is shown. Figure 4The analysis shows that the high entropy carbide precursor xerogel undergoes chemical fracture after high temperature pyrolysis. The pyrolysis yield can be obtained to be about 45-55% by comparing the mass before and after pyrolysis.

[0092] Structure and performance characterization of prepared transition metal carbide high entropy ceramics

[0093] The high entropy carbides prepared in Examples 2, 3, 4, and 5 were subjected to XRD tests. The test results are shown in FIG. Figure 5 As shown, from Figure 5 It can be seen that the high-angle main crystal phase of the dense nano-transition metal carbide high-entropy ceramic prepared by the method provided by the present invention is NbC.

[0094] The transition metal carbide high entropy ceramics prepared in Example 4 were subjected to high-resolution TEM testing. The test results are as follows: Figure 6 As shown in the figure, it can be seen that the elements are evenly distributed and the grain size distribution ranges from 70 to 80 nm.

[0095] The high entropy carbide ceramics obtained in Examples 1-4 above were subjected to relative density and porosity tests, and the specific results are shown in Table 1.

[0096] Table 1 Performance parameters of Examples 1-4

[0097]

[0098] Note: Relative density refers to the ratio of actual density to theoretical density of transition metal carbide high entropy ceramics.

[0099] As can be seen from Table 1, Examples 1 to 4 can produce high-quality transition metal carbide high-entropy ceramics mainly due to the high temperature and high pressure used in the SPS sintering process, which can inhibit atomic diffusion and grain coarsening, promote single-phase carbide solid solution, and make the prepared high-entropy carbide ceramics dense. The high-entropy carbide ceramic target prepared in Examples 1 to 4 has a density of 95.09%-99.86%; the tube furnace pyrolysis precursor process is used to allow the in-situ reaction in the high-entropy carbide precursor powder to occur completely, and the rapid sintering will inhibit grain growth, and control its grain size in the range of 70-80nm.

[0100] Therefore, the high entropy carbide ceramic prepared by the present invention has high density and nano-scale grain size, and is widely used in the fields of radiation resistance and thermal protection. The method described in the present application is simple to operate, has a short production cycle, and has a wide range of applications.

[0101] In summary, the preparation method of transition metal carbide high entropy ceramics provided by the present invention, the holding temperature of the high temperature cracking precursor has a great influence on the grain size of the high entropy carbide ceramics and the final uniformity of the composition; spark plasma sintering, as a field-assisted sintering process, has the advantages of uniform heating, high heating rate, low sintering temperature, short sintering time, controllable organizational structure, and high production efficiency. Therefore, the embodiment of the present invention can achieve rapid sintering, reduce energy consumption, and make the prepared high entropy carbide ceramics have a density of 95.09%-99.86%, uniform composition, and an adjustable grain size range of ≥70nm.

[0102] The above are only preferred embodiments of the present application and are not intended to limit the present application. It should be understood that for those skilled in the art, many modifications and changes can be made according to the concept of the present application without creative work, and improvements and transformations can be made according to the concept of the present application. Any modifications, equivalent substitutions, improvements, etc. made, all of which should fall within the scope of protection of the rights attached to the present application. Therefore, any technical solution that can be obtained through logical analysis, reasoning or limited experiments based on the concept of the present application on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing dense nano transition metal carbide high entropy ceramics, characterized in that: The following steps are involved: (1) mixing a transition metal salt and a carbon source in an organic solvent at 50-70° C. and stirring to obtain a high entropy carbide precursor wet gel; The transition metal salt and the carbon source are measured according to a molar ratio of transition metal to carbon of (1.2-1):(1-5); (2) The high entropy carbide precursor wet gel is dried to obtain a high entropy carbide precursor dry gel; (3) grinding the obtained high entropy carbide precursor dry gel into powder, and then pyrolyzing it under a protective atmosphere; (4) The pyrolyzed powder is spark plasma sintered at 1900-2000°C to obtain dense nano-transition metal carbide high entropy ceramics.

2. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 1, characterized in that: In step (1), the transition metal salt comprises at least one transition metal chloride; the transition metal is selected from Ti, Nb, Ta, Cr, Mo, Zr, W, V or Hf.

3. The method for preparing the dense nano transition metal carbide high entropy ceramic according to claim 2, characterized in that: The transition metal salt includes three or more transition metal chlorides.

4. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 1, characterized in that: The carbon source is at least one of furfuryl alcohol, starch and sucrose.

5. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 1, characterized in that: The organic solvent is ethanol.

6. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 1, characterized in that: In step (2), the high entropy carbide precursor wet gel is dried at 100-170° C. to obtain a high entropy carbide precursor dry gel, and the heat preservation time is 12-18 hours.

7. The method for preparing the dense nano transition metal carbide high entropy ceramic according to claim 1 or 6, characterized in that: In step (3), the pyrolysis temperature of the high entropy carbide precursor dry gel is 1000-1600° C., and the pyrolysis temperature insulation time is 1-2 h; the protective atmosphere used is argon or nitrogen.

8. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 7, characterized in that: In step (4), the cracked powder is first ball milled and then spark plasma sintered.

9. The method for preparing dense nano transition metal carbide high entropy ceramics according to claim 8, characterized in that: Spark plasma sintering at ≤5×10 -2 Under the vacuum degree of Pa, the heating or cooling rate is 50-100℃ / min, which is divided into 2 to 3 gradient heating or cooling steps. After heating to the set maximum temperature, it is kept warm for 10-25min; the spark plasma sintering pressure is 40-65MPa.

10. The dense nano-transition metal carbide high entropy ceramic prepared by the method according to any one of claims 1 to 9, wherein the grain size is 70-80 nm; the porosity is 0-5%, excluding the end value 0; and the density is greater than 95%.

Citation Information

Patent Citations

  • High-entropy carbide nano-powder and preparation method thereof

    CN110104648A

  • High-purity ultrafine transition metal carbide single-phase high-entropy ceramic powder and preparation method thereof

    CN110330341A

  • Method for refining transition high-entropy carbide ceramic grains

    CN116947496A

  • Low-temperature preparation method of single-phase multi-principal-element ultra-high-temperature ceramic nano-powder