Preparation method of boron carbide / diamond composite bulletproof material

By adding diamond particles and sintering aids to boron carbide ceramics and using SPS sintering technology, the problems of difficult sintering and poor fracture toughness of boron carbide ceramics are solved, and its density, hardness and toughness are improved, meeting the high performance of ceramic bulletproof materials. need.

CN118754694APending Publication Date: 2024-10-11HENAN UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202411059124.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Boron carbide ceramic materials are difficult to sinter in the field of protection, have poor fracture toughness, poor impact resistance, and low density, which limits their application.

Method used

The boron carbide diamond composite ceramic preparation method is adopted, by selecting diamond particles as the second phase reinforcement material, adding sintering aids such as silicon, titanium and their carbides, and using SPS sintering technology and grinding and polishing processes to improve the density, hardness and toughness of the material. .

Benefits of technology

The density, hardness and fracture toughness of boron carbide diamond composite ceramics are significantly improved, which is suitable for ceramic bulletproof requirements and meets the requirements of high hardness, high toughness and high strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a high-strength and high-toughness boron carbide diamond composite ceramic bulletproof sheet and a preparation method thereof, and belongs to the field of composite ceramic protection. Required materials comprise boron carbide, diamond, silicon, titanium and other sintering aids. The preparation method comprises the steps of material mixing, pressing, SPS sintering, grinding and polishing and detection. Wherein the proportion of the diamond is 10 to 30 wt%, the proportion of the boron carbide is 60 to 75 wt%, and the proportion of the sintering aid is 8 to 20 wt%; the particle size of the boron carbide is 2-4 [mu] m, and the particle size of the diamond is 1-45 [mu] m. The prepared boron carbide diamond composite ceramic chip is small in density, high in hardness and good in toughness. The surface of the diamond is graphitized at high temperature and reacts with silicon to generate silicon carbide, so that the compactness of a sample is better. The composite bulletproof ceramic prepared by the invention has greatly improved hardness, toughness and bending strength, is suitable for bulletproof field requirements, and has high application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention patent relates to the field of composite ceramic bulletproof technology, and specifically to a method for preparing a high-strength and high-toughness composite bulletproof ceramic of boron carbide diamond. Background Art

[0002] At present, commonly used armor protection materials include metal armor materials, such as armor steel, and non-metal armor materials, such as ceramics. For bulletproof armor and bulletproof equipment, bulletproof materials should meet the requirements of "high hardness, high toughness, high strength, and low density" as much as possible. Compared with traditional metal protective equipment, ceramic protective materials have low density and light weight. The main ceramic materials used in the field of protection are boron carbide, silicon carbide, alumina ceramics and their composite materials. The famous American armed helicopter AH-64A uses composite ceramics as bulletproof armor, and its "Interceptor" bulletproof vest uses composite ceramic bulletproof inserts on the chest and back. Among the main tanks, the current German Leopard-II, the British Challenger series, the Israeli Merkava, the American Abrams (MI), EE-T1 Osorio, the Soviet T-72 and other main battle tanks are equipped with carbide ceramic composite armor on their top, bottom and sides. In the 1960s, boron carbide ceramics were installed on the cockpit floors, side wall bulletproof panels and pilot seats of my country's armed helicopters. In 2016, bulletproof ceramic armor plates were installed on the cockpit and shoulders of the Chinese Army Aviation Z-10, which can withstand the impact of 12.7 mm large-caliber machine gun bullets.

[0003] Among the above ceramic materials, boron carbide materials have been widely used in the field of protection due to their high hardness, low density, high melting point and other characteristics, such as armored vehicles, tanks, helicopters and bulletproof vests. However, due to the characteristics of the strong covalent bond structure of boron carbide, it is difficult to sinter, and it is highly resistant to grain boundary sliding and lacks plasticity. The densification of stoichiometric boron carbide is very difficult, resulting in poor fracture toughness, poor impact resistance and low density after sintering, which greatly limits the application of boron carbide ceramic materials in the field of protection.

[0004] In order to improve the mechanical properties of boron carbide ceramics after sintering, the commonly used method is to add second phase particles to strengthen and toughen them into composite materials. For boron carbide, the most commonly used method is to add carbon sources, such as diamond, carbon black, etc. Among them, diamond has the best effect on improving the hardness and toughness of boron carbide, and has little effect on density. Summary of the invention

[0005] In view of the improvement of mechanical properties in the above background technology, the purpose of the present invention is to provide a method for preparing boron carbide diamond composite ceramics to solve the problems of low hardness and poor toughness of composite ceramics in the prior art. Technical Solution

[0006] To achieve the above object, the technical solution of the present invention is as follows: A method for preparing a boron carbide diamond composite bulletproof material comprises the following steps: Step 1: Raw material selection, wherein the main ceramic phase is 80-90 wt%, the sintering aid is 8-20 wt%, and the dispersant is 0.1-2 wt%.

[0007] Furthermore, in step 1, the main ceramic phases are diamond and boron carbide, the mass fraction of diamond is 10-30%, the mass fraction of boron carbide is 60-75%, the diamond particle size is 1-45 μm, the boron carbide particle size is 2-4 μm, and the purity of the diamond powder and boron carbide is ≥99.99%.

[0008] Furthermore, the sintering aid in step 1 is one or a mixture of silicon, titanium and its carbides and rare earth oxides, and the silicon and titanium compounds are selected from one or a mixture of two or more of silicon carbide, titanium carbide, titanium dioxide and titanium boride, and the purity of silicon, titanium and its carbides is ≥99.9%.

[0009] Step 2: Mixing: Mix the main ceramic phase and the sintering aid according to a certain proportion, stir evenly, and place the obtained mixed slurry in a vacuum drying oven to dry.

[0010] Furthermore, in step 2, the mixing is carried out in a ball mill, anhydrous ethanol is used as the solvent, zirconium oxide balls are selected, the mass ratio of material: solvent: ball is 1:1:4, the mixing time is 10 h, the drying temperature is 60°C, and the drying time is 12 h.

[0011] Step 3: Sintering of diamond particle reinforced boron carbide composite material, pre-pressing before sintering, SPS sintering.

[0012] Furthermore, in step three, the SPS sintering has a pressure of 40-50 MPa, a sintering temperature of 1400-1700 °C, a vacuum degree of less than or equal to 10 Pa, a holding time of 5-15 min, a heating rate of 100 °C / min+75 °C / min+50 °C / min, carbon paper and carbon sheets are placed on the upper and lower parts of the powder, carbon felt is used to insulate the mold, and the mold is a graphite mold.

[0013] Step 4: Grinding and polishing. After taking out the ceramic sample, first roughly grind off the upper and lower layers of carbon paper, then polish, roughly polish until it is flat, and then fine polish.

[0014] Furthermore, in step 4, a grinding and polishing process is performed, wherein a diamond grinding wheel is used for the rough grinding, a veneer cloth or a woolen cloth is used for the rough polishing, a silk cloth is used for the fine polishing, the polishing agent is a diamond polishing agent, and the polishing machine speed is 620 r / min.

[0015] Step 5: Testing: After polishing, the composite bulletproof ceramic sheet of the present invention is obtained and tested.

[0016] Beneficial effects of the present invention: The present invention selects diamond particles as the second phase reinforcement material, and the prepared boron carbide diamond composite ceramic sheet has low density, high hardness and good toughness. The sintering aids silicon and titanium react with the partially graphitized carbon on the surface of the diamond during the reaction process to produce silicon carbide, titanium carbide and other enhanced composite ceramic materials toughness, making the performance more superior, especially reflected in the fracture toughness, and in-situ generation of silicon carbide and titanium carbide, making the sample more compact, reducing pores, and having better density. The boron carbide diamond composite material prepared by the present invention has greatly improved density, hardness, fracture toughness and flexural strength of the sample finally obtained, which is fully suitable for the needs of ceramic bulletproof. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with specific embodiments: Example

[0018] A boron carbide diamond composite bulletproof ceramic is composed of the following raw materials, measured by mass percentage: 20% diamond powder, 60% boron carbide, 15% silicon powder, 5% titanium powder, and a dispersant.

[0019] According to the above ratio, the raw materials were weighed, diamond powder (1-10 μm) was mixed with boron carbide (2-4 μm), silicon powder (1-3 μm), titanium powder (300 mesh), and dispersant with anhydrous ethanol, and the mass ratio of zirconium oxide balls was 1:1:4. The mixing time was 10 h, the drying temperature was 60 °C, and the mixed powder was obtained after the drying time was 12 h. The mixed powder was weighed according to the mass obtained by the theoretical density of the composite ceramic material and the volume of the graphite mold, and then pre-pressed with a mold, the pre-pressing time was 5 min, the pressure was 50 MPa, the sintering temperature was 1500 °C, the vacuum degree was less than or equal to 10 Pa, the insulation time was 15 min, the heating rate was 100 °C / min+50 °C / min, carbon paper and carbon sheet were placed on the upper and lower parts of the powder, and carbon felt was used to insulate the mold, and finally the desired boron carbide diamond composite ceramic was obtained.

[0020] The composite superhard bulletproof ceramic prepared in this embodiment has a Vickers hardness of 36.3 GPa and a fracture toughness of 4.18 MPa.m 1 / 2 , flexural strength is 351 MPa, density is 2.53 g / cm 3 , the density is 94.3%.

[0021] Embodiment 2: A boron carbide diamond composite bulletproof ceramic is composed of the following raw materials, measured by mass percentage: 20% diamond powder, 60% boron carbide, 15% silicon powder, 5% titanium powder, and a dispersant.

[0022] The raw materials were weighed according to the above ratio, and diamond powder (1-10 μm) was mixed with boron carbide (2-4 μm), silicon powder (1-3 μm), titanium powder (300 mesh), and dispersant with anhydrous ethanol. The material: solvent: ball mass ratio was 1:1:4, the mixing time was 10 hours, the drying temperature was 60 °C, and the mixed powder was obtained after the drying time was 12 hours. The mixed powder was weighed according to the mass obtained by the theoretical density of the composite ceramic material and the volume of the graphite mold, and then pre-pressed with a mold, the pre-pressing time was 5 min, the pressure was 50 MPa, the sintering temperature was 1550 °C, the vacuum degree was less than or equal to 10 Pa, the insulation time was 15 min, the heating rate was 100 °C / min +50 °C / min, carbon paper and carbon sheet were placed on the upper and lower parts of the powder, and carbon felt was used to insulate the mold, and finally the desired boron carbide diamond composite ceramic was obtained.

[0023] The composite superhard bulletproof ceramic prepared in this embodiment has a Vickers hardness of 35.9 GPa and a fracture toughness of 5.19 MPa.m 1 / 2 , flexural strength is 357 MPa, density is 2.56 g / cm 3 , the density is 94.8%.

[0024] Embodiment 3: A boron carbide diamond composite bulletproof ceramic is composed of the following raw materials, measured by mass percentage: 20% diamond powder, 60% boron carbide, 12% silicon powder, 5% titanium powder, 3% lanthanum oxide, and a dispersant.

[0025] According to the above ratio, the raw materials were weighed, diamond powder (1-10 μm) was mixed with boron carbide (2-4 μm), silicon powder (1-3 μm), titanium powder (300 mesh), and dispersant with anhydrous ethanol, and the mass ratio of zirconium oxide balls was 1:1:4. The mixing time was 10 h, the drying temperature was 60 °C, and the mixed powder was obtained after the drying time was 12 h. The mixed powder was weighed according to the mass obtained by the theoretical density of the composite ceramic material and the volume of the graphite mold, and the mold was pre-pressed for 5 min, the pressure was 50 MPa, the sintering temperature was 1550 °C, the vacuum degree was less than or equal to 10 Pa, the holding time was 15 min, the heating rate was 100 °C / min+75 °C / min+50 °C / min, carbon paper and carbon sheet were placed on the upper and lower parts of the powder, and carbon felt was used to keep the mold warm, and finally the desired boron carbide diamond composite ceramic was obtained.

[0026] The composite superhard bulletproof ceramic prepared in this embodiment has a Vickers hardness of 37.2 GPa and a fracture toughness of 6.43 MPa.m 1 / 2 , flexural strength is 361 MPa, density is 2.57 g / cm 3 , the density is 95.2%.

[0027] Comparative Example: A boron carbide diamond composite bulletproof ceramic is composed of the following raw materials in percentage by mass: 10% diamond powder, 85% boron carbide and 5% titanium powder.

[0028] According to the above ratio, the raw materials were weighed, diamond powder (1-10 μm) and boron carbide (4-5 μm) titanium powder (300 mesh) were mixed evenly with anhydrous ethanol, zirconium oxide balls, material: solvent: ball mass ratio of 1:1:4, mixing time of 10 h, drying temperature of 60 ℃, drying time of 12 h to obtain mixed powder. The mixed powder was weighed according to the mass obtained by the theoretical density of the composite ceramic material and the volume of the graphite mold, and then pre-pressed with a mold, pre-pressing time of 5 min, pressure of 50 MPa, sintering temperature of 1550 ℃, vacuum degree less than or equal to 10 Pa, insulation time of 15 min, heating rate of 100 ℃ / min, carbon paper and carbon sheet were placed on the upper and lower parts of the powder, and carbon felt was used to keep the mold warm, and finally the desired boron carbide diamond composite ceramic was obtained.

[0029] The composite superhard bulletproof ceramic prepared in this comparative example has a Vickers hardness of 35.56 GPa and a fracture toughness of 4.62 MPa.m 1 / 2 , flexural strength is 349 MPa, density is 2.31 g / cm 3 The density is 88.71% and there are many pores.

[0030] Through the results of the examples and comparative examples, it can be seen that the addition of silicon can stabilize the surface of diamond particles to react more graphite phases, and the in-situ generation of liquid silicon carbide penetrates between diamond particles under sintering at a temperature higher than the melting point of silicon (1410 ° C), thereby enhancing the bonding of diamond particles in the composite material. The introduction of titanium enhances the interface bonding between diamond and boron carbide and covers the diamond. The introduction of lanthanum oxide generally improves the sintering performance and density. Compared with the comparative example, the density in the example is increased by 6.49%.

[0031] Finally, it should be noted that the above description is only a preferred embodiment during SPS sintering and is not intended to limit the present invention.

Claims

1. A method for preparing a boron carbide diamond composite bulletproof material, characterized in that: The following steps are involved: (1) Raw material selection: main ceramic phase 80-90 wt%, sintering aid 8-20 wt%, dispersant 0.1-2 wt%; (2) Mixing: The main ceramic phase and the sintering aid are mixed in proportion, and the resulting mixed slurry is placed in a vacuum drying oven for drying; (3) Sintering: pre-pressing before sintering, SPS sintering, and taking out after cooling to room temperature to obtain a boron carbide diamond composite bulletproof ceramic sheet; (4) Grinding and polishing: After taking out the ceramic sample, first roughly grind off the upper and lower layers of carbon paper, then polish, roughly polish until it is flat, and then fine polish; (5) Testing: After polishing, the composite bulletproof ceramic sheet of the present invention is obtained and tested.

2. The boron carbide diamond composite bulletproof ceramic raw material selection according to claim 1, characterized in that: The main ceramic phase is 10-30 wt% diamond and 60-75 wt% boron carbide, and the sintering aid is one or a mixture of silicon, titanium and its compounds and rare earth oxides.

3. The boron carbide diamond composite bulletproof ceramic mixture according to claim 1, characterized in that: The materials were mixed in a ball mill, anhydrous ethanol was used as the solvent, zirconia balls were selected, the mass ratio of material: solvent: ball was 1:1:4, the mixing time was 10 h, the drying temperature was 60 °C, and the drying time was 12 h.

4. The boron carbide diamond composite bulletproof ceramic sintering according to claim 1, characterized in that: During the sintering process, the pressure is 40-50 MPa, the sintering temperature is 1400-1700 ℃, the vacuum degree is less than or equal to 10 Pa, the holding time is 5-15 min, the heating rate is 100 ℃ / min+75 ℃ / min+50 ℃ / min, carbon paper and carbon sheets are placed on the upper and lower parts of the powder, carbon felt is used to insulate the mold, and the mold is a graphite mold.

5. The grinding and polishing method of boron carbide diamond composite bulletproof ceramic according to claim 1, characterized in that: The rough grinding uses a diamond grinding disc, the rough polishing uses a veneer cloth or a woolen cloth, the fine polishing uses a silk cloth, the polishing agent is a diamond polishing agent, and the polishing machine rotates at a speed of 620 r / min.

6. The main ceramic phase selection according to claim 2, characterized in that: The particle size of boron carbide is 2-4 μm, the particle size of diamond is 1-45 μm, and the purity of diamond powder and boron carbide is ≥99.99%.

7. The sintering aid selection according to claim 2, characterized in that: The sintering aid silicon and titanium compounds are selected from one or a mixture of two or more of silicon carbide, titanium carbide, titanium dioxide and titanium boride, and the rare earth oxide is selected from lanthanum oxide. The purity of the silicon, titanium and their carbides is ≥99.9%.

Citation Information

Patent Citations

  • Boron carbide silicon carbide composite ceramic and preparation method thereof

    CN103030396A

  • Ultra-hard ceramic bulletproof piece and preparation method thereof

    CN105272268A

  • Boron carbide-based composite ceramic material with linear conductivity and preparation method thereof

    CN111410537A

  • Preparation method of boron carbide and diamond combined composite superhard bulletproof ceramic

    CN117486613A

  • Boron carbide sintered body and protective member

    US20070203012A1

Cited By

  • A precursor-derived nanocrystalline boron carbide-based composite ceramic and a superhigh-pressure preparation method thereof

    CN122916677A