Anti-swelling high-strength high-toughness conductive material and preparation method thereof

By introducing quaternary ammonium salts and nanosheets into the hydrogel, a composite film is formed, and multiple interactions are used to improve the mechanical properties, solving the problem that the hydrogel is easy to break after saturated swelling, and achieving swelling resistance, high strength and high toughness. Preparation of conductive hydrogel materials suitable for multifunctional material applications.

CN118755220APending Publication Date: 2024-10-11CHANGCHUN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410913509.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing hydrogels are prone to fracture after saturated swelling, resulting in reduced mechanical strength and service life. It is difficult to develop materials with high mechanical strength without sacrificing maximum extensibility and toughness.

Method used

A method for preparing a conductive material that is resistant to swelling, has high strength and high toughness, and adds glycidyltrimethylammonium chloride, sodium hydroxide, dilute hydrochloric acid, polydopamine nanosheets and 3,4-dihydroxy to the polyvinyl alcohol aqueous solution. Benzaldehyde forms a composite film that utilizes the cation-π interaction between the quaternary ammonium salt and DBA and the hydrogen bonding between the hydroxyl group of PVA and catechol and polydopamine nanosheets to improve the mechanical properties.

Benefits of technology

The mechanical properties and anti-swelling properties of the composite membrane are significantly improved, allowing the material to maintain resilience after long-term contact with water. It has high mechanical strength and toughness and is suitable for the preparation of multifunctional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755220A_ABST
    Figure CN118755220A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of hydrogel preparation, and relates to an anti-swelling high-strength high-toughness conductive material and a preparation method thereof.The preparation method comprises the following steps that a glycidyl trimethyl ammonium chloride aqueous solution and a sodium hydroxide aqueous solution are added into a polyvinyl alcohol aqueous solution, a reaction is conducted for 2-4 h at the temperature of 70-90 DEG C, and then diluted hydrochloric acid is added to stop the reaction; adding a polydopamine nanosheet aqueous solution into the obtained solution, and carrying out stirring reaction at 60-80 DEG C for more than 6 hours; 3, 4-dihydroxybenzaldehyde and diluted hydrochloric acid are added into the obtained solution, stirring reaction is conducted at the temperature of 60-80 DEG C, the solution is cooled to the room temperature and poured into a mold, drying is conducted in a drying oven at the temperature of 35-45 DEG C, and the solvent is volatilized to form the film. According to the hydrogel prepared by the preparation method disclosed by the invention, the mechanical property of a compound film is remarkably improved by utilizing multiple interactions among substances, so that the compound material has the mechanical property suitable for nervous tissues and transmits an electric signal through electric conduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogel preparation, and relates to a swelling-resistant, high-strength and high-toughness conductive material and a preparation method thereof. Background Art

[0002] Hydrogels are soft materials formed by physical or chemical crosslinking, and their microstructure is a three-dimensional network. Hydrogels can absorb a large amount of water. The water absorption and swelling characteristics of hydrogels are also an important factor affecting the performance of materials. As the amount of water absorbed by the hydrogel increases, its volume will expand rapidly. After reaching saturated swelling, many hydrogels will become fragile and easy to break due to the accumulation of internal stress, thereby reducing their mechanical strength and service life. To solve the problem of easy breakage of hydrogels after saturated swelling, the representative strategy is to introduce energy dissipation mechanisms, such as introducing sliding or sacrificial bonds and reversible crosslinking in a single network structure to dissipate energy. Examples of the latter include metal coordination, hydrogen bonding, supramolecular systems, and ionic or Coulomb interactions, thereby forming a double network to achieve energy dissipation, induce dense crystalline domains, and create supramolecular interactions. In addition, the use of structural engineering methods, such as by creating ordered nanostructures in hydrogels, such as mechanical training, directional freezing, and hydrogen bonding interactions, is also a way to regulate the mechanical properties of hydrogel materials. In the field of tissue repair, anti-swelling hydrogels can maintain a stable volume, reduce the extrusion of surrounding normal nerve tissue, and reduce potential continued damage. Despite the high demand for tough, high-modulus polymer materials, it remains difficult to develop strategies to develop hydrogel materials with high mechanical strength without sacrificing their maximum extensibility and toughness. Summary of the invention

[0003] The present invention aims to provide a conductive material that is resistant to swelling and has good mechanical properties and a preparation method thereof, in view of the shortcomings of the prior art that most materials are prepared by a blending method and the prepared materials have poor functionality.

[0004] The technical solution adopted by the present invention to solve the technical problem is:

[0005] The present invention provides a method for preparing a conductive material with high swelling resistance, high strength and high toughness, comprising the following steps:

[0006] Step 1: Add glycidyl trimethylammonium chloride aqueous solution and sodium hydroxide aqueous solution to the polyvinyl alcohol aqueous solution, react at 70-90° C. for 2-4 hours, and then add dilute hydrochloric acid to terminate the reaction;

[0007] Step 2: Add the polydopamine nanosheet aqueous solution to the solution obtained in step 1, and stir the mixture at 60-80° C. for more than 6 hours;

[0008] Step 3: Add 3,4-dihydroxybenzaldehyde and dilute hydrochloric acid to the solution obtained in step 2, and stir at 60-80° C. for 8-12 hours;

[0009] Step 4: The solution is cooled to room temperature, poured into a mold, and dried in an oven at 35-45°C to evaporate the solvent and form a film;

[0010] The molar ratio of the polyvinyl alcohol, glycidyl trimethyl ammonium chloride, polydopamine nanosheets and 3,4-dihydroxybenzaldehyde is 0.02-0.04: 11.3-22.6: 0.48-0.92: 0.29-0.58.

[0011] Furthermore, the polyvinyl alcohol is M w The polyvinyl alcohol is preferably 40000 to 120000. w =Polyvinyl alcohol of 97000, 47000, 67000, 75000, 82000, and 105000.

[0012] Furthermore, in step 1, the concentration of the polyvinyl alcohol aqueous solution is 0.0005 mol / L to 0.001 mol / L.

[0013] Furthermore, the concentration of glycidyl trimethylammonium chloride in step 1 is 1.13 mol / L to 2.26 mol / L.

[0014] Furthermore, the amount of dilute hydrochloric acid in step 1 is 0.05 to 0.1 times that of glycidyl trimethylammonium chloride.

[0015] Furthermore, the concentration of the polydopamine nanosheet aqueous solution in step 2 is 0.012 mol / L to 0.024 mol / L.

[0016] Furthermore, in step three, the amount of the dilute hydrochloric acid substance is 1.6 to 1.8 times that of 3,4-dihydroxybenzaldehyde.

[0017] Furthermore, in step 1, the concentration of the sodium hydroxide aqueous solution is 4wt% to 7wt%.

[0018] Furthermore, the concentration of the dilute hydrochloric acid in step 1 and step 3 is 0.5 mol / L to 1.5 mol / L.

[0019] The hydrogel prepared by the present invention has developed a conductive hydrogel film with high elastic modulus and anti-swelling by a one-step molding technology. The quaternary ammonium salt itself carries anions and cations, and can form cation-π interactions with the catechol structure on DBA, and the hydroxyl on PVA forms hydrogen bonds with catechol and polydopamine nanosheets. Due to the introduction of the quaternary ammonium group, the hydrophilicity of the composite film is greatly increased. It is worth noting that the composite film can still maintain resilience after being in contact with water for a long time. The multiple interactions between substances are utilized to significantly improve the mechanical properties of the composite film.

[0020] The advantages and positive effects of the present invention are:

[0021] The present invention utilizes polyvinyl alcohol to contain a large number of hydroxyl groups, which is easy to functionalize and modify. By selecting simple and efficient methods such as acetalization reaction and epoxy ring opening, catechol and quaternary ammonium group cations are introduced into the PVA material, and more importantly, the polydopamine nanosheets are cleverly introduced into the composite system. The cation-π interaction between glycidyl trimethyl ammonium chloride and 3,4-dihydroxybenzaldehyde can give the system dynamic and spatial configurability, while forming small crystal domains, promoting crystal orientation and achieving effective energy dissipation. The nanosheets with a two-dimensional structure have a high specific surface area and high surface energy, can effectively enhance the loading and transfer of the PVA matrix, and improve its tensile resistance. The two-dimensional nanosheet has a good crystallization auxiliary effect as a crystal nucleus, can promote the crystallization behavior of PVA, and improve its crystallinity and crystallization rate. In addition, the catechol structure exists in the polydopamine nanosheet, so that the polydopamine nanosheet, 3,4-dihydroxybenzaldehyde and glycidyl trimethyl ammonium chloride all have hydrogen bond interactions with polyvinyl alcohol, so that the polymer has excellent mechanical properties. At the same time, the material has a certain conductivity and can transmit electrical signals. It is worth noting that the polymer material has good anti-swelling properties after long-term contact with water. The material has a certain mechanical strength in water. The preparation method adopts a one-pot method. The whole process reduces the cycle and cost. The prepared new multifunctional material has good mechanical properties. The new multifunctional material has broad application prospects in the fields of sensing and detection, flexible electronic and optoelectronic devices, and tissue engineering repair scaffolds. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the preparation method of the PVA composite film;

[0023] Figure 2 The following are Fourier transform infrared spectra of the films of Example 1, Comparative Examples 1-3 and pure PVA;

[0024] FIG3( a ) is a tensile stress-strain curve of Example 1, Comparative Examples 1-3 and pure PVA;

[0025] FIG3( b ) shows the elastic modulus and toughness of Example 1, Comparative Examples 1-3 and pure PVA;

[0026] FIG4( a ) is a tensile stress-strain curve of the hydrogel wet films prepared in Example 1 and Examples 4-6;

[0027] FIG4( b ) is a tensile stress-strain curve of the hydrogel dry films prepared in Example 1 and Examples 4-6;

[0028] Figure 5 (a) shows 10 consecutive loading-unloading cycles of the wet film of PVA / GTMAC / PDA / DBA hydrogel in Example 1 at room temperature;

[0029] Figure 5(b) shows the loading-unloading cycle of the PVA / GTMAC / PDA / DBA hydrogel wet film of Example 1 at different strains at room temperature;

[0030] Figure 6 The water absorption and swelling behavior of the PDA-8 hydrogel film prepared in Example 4. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0032] Swelling behavior test method:

[0033] The hydrogel film was placed in a dish with a diameter of 70 mm and filled with water. The film was weighed at fixed time points and the size changes after 3 and 7 days were observed. The swelling behavior was calculated based on the weight change between the equilibrium state and the dry state at different swelling times as follows: Water content = (m swollen -m dry / m swollen )×100%

[0034] Among them, m dry is the mass of the hydrogel sample dried at 60 °C for 3 hours, m swollen To balance the mass of the hydrogel.

[0035] Conductivity test: Cut the film into a rectangular film with a length of 1 cm, a width of 0.5 cm, and a thickness of about 2 mm. Connect the two ends of the probe to the two ends of the film and read the resistance value. The conductivity calculation formula is:

[0036]

[0037] Where L is the film length, R is the resistance, and A is the cross-sectional area.

[0038] Strength and toughness test methods:

[0039] The tensile tests were performed at room temperature using a multifunctional testing machine (QJ211S, Shanghai) with a 100N load cell. The hydrogel films were cut into dumbbell shapes with a width of 4 mm. The thickness of each hydrogel film sample was carefully measured with a caliper. Unless otherwise stated, the stretching speed was kept at 10 mm / min. The elastic modulus was calculated from the linear slope of the elastic region between strains in the stress-strain curve. The toughness was calculated based on the area under the stress-strain curve. For the cyclic tensile test, the hydrogel film samples were repeatedly loaded to a certain strain and then unloaded at the same strain rate without any rest time. The hydrogel film samples were loaded to different strains and unloaded at the same strain rate without any rest time.

[0040] Example 1

[0041] Preparation of PVA / GTMAC / PDA / DBA: w =97000 (2g, 0.02mmol) was added to a round-bottom flask with 40mL of deionized water and stirred at 90℃ for 2h until the polyvinyl alcohol was completely dissolved. The temperature was set to 80℃, and 10mL of deionized water-dissolved glycidyl trimethylammonium chloride (1.72g, 11.3mmol) was added, and 5% sodium hydroxide solution was added and heated and stirred for 3h. Dilute hydrochloric acid (1M) was added to terminate the reaction. The reaction temperature was adjusted to 70℃, and 4mL of 0.012mol / L polydopamine nanosheet aqueous solution was added, and the reaction was stirred for more than 6h. At 70℃, 3,4-dihydroxybenzaldehyde (0.04g, 0.29mmol) was added, and dilute hydrochloric acid (1M) was added, and the reaction was stirred overnight. The solution was cooled to room temperature, poured into a mold, dried in an oven at 35℃, and the solvent evaporated to form a film, which was recorded as PDA-4.

[0042] Example 2

[0043] Preparation of PVA / GTMAC / PDA / DBA: Add polyvinyl alcohol Mw=97000 (3g, 0.03mmol) to a round-bottom flask with 40mL deionized water and stir at 90℃ for 2h until the polyvinyl alcohol is completely dissolved. Set the temperature to 80℃, add 10mL of deionized water dissolved trimethyl ammonium chloride (2.58g, 16.95mmol), add 5wt% sodium hydroxide solution and heat and stir for 3h. Add dilute hydrochloric acid (1M) to terminate the reaction. Adjust the reaction temperature to 70℃, add 4mL 0.018mol / L polydopamine nanosheet aqueous solution, and stir the reaction for more than 6h. At 70℃, continue to add 3,4-dihydroxybenzaldehyde (0.06g, 0.435mmol), add dilute hydrochloric acid (1M), and stir the reaction overnight. Cool the solution to room temperature, pour it into a mold, dry it in an oven at 35℃, and the solvent evaporates to form a film.

[0044] Example 3

[0045] Preparation of PVA / GTMAC / PDA / DBA: Add polyvinyl alcohol Mw=97000 (4g, 0.04mmol) to a round-bottom flask with 40mL deionized water, stir at 90℃ for 2h until the polyvinyl alcohol is completely dissolved. Set the temperature to 80℃, add 10mL of deionized water dissolved trimethyl ammonium chloride (3.44g, 22.6mmol), add 5wt% sodium hydroxide solution and heat and stir for 3h. Add dilute hydrochloric acid (1M) to terminate the reaction. Adjust the reaction temperature to 70℃, add 4mL 0.024mol / L polydopamine nanosheet aqueous solution, and stir the reaction for more than 6h. At 70℃, continue to add 3,4-dihydroxybenzaldehyde (0.08g, 0.58mmol), add dilute hydrochloric acid (1M), and stir the reaction overnight. Cool the solution to room temperature, pour it into a mold, dry it in an oven at 35℃, and the solvent evaporates to form a film.

[0046] Example 4

[0047] The difference from Example 1 is that 8 mL of 0.012 mol / L polydopamine nanosheet aqueous solution is added, and the prepared membrane is denoted as PDA-8.

[0048] After immersing PDA-8 in water for 3 days, its size did not increase significantly. Figure 6 The real-time swelling curves in Figure 2 show that the water content of PDA-8 in deionized water remains almost unchanged at about 79 wt% within 3 days, and the size of the sample remains almost unchanged after being immersed in water for 7 days, indicating that the polymer membrane has good anti-swelling properties.

[0049] Example 5

[0050] The difference from Example 1 is that 12 mL of 0.012 mol / L polydopamine nanosheet aqueous solution is added, and the prepared membrane is denoted as PDA-12.

[0051] Example 6

[0052] The difference from Example 1 is that 16 mL of 0.012 mol / L polydopamine nanosheet aqueous solution is added, and the prepared membrane is denoted as PDA-16.

[0053] Comparative Example 1

[0054] Preparation of PVA / GTMAC: Polyvinyl alcohol M w=97000 (2g, 0.02mmol) was added to a round-bottom flask with 40mL of deionized water and stirred at 90℃ for 2h until the polyvinyl alcohol was completely dissolved. The temperature was set to 80℃, and 10mL of deionized water dissolved glycidyl trimethylammonium chloride (1.72g, 11.3mmol) was added, and 5% sodium hydroxide solution was added and heated and stirred for 3h. Dilute hydrochloric acid (1M) was added to terminate the reaction. The solution was cooled to room temperature, poured into a mold, and dried in an oven at 35℃ to evaporate the solvent to form a film.

[0055] Comparative Example 2

[0056] Preparation of PVA / DBA: w =97000 (2 g, 0.02 mmol) was added to a round-bottom flask with 40 mL of deionized water and stirred at 90 ° C for 2 h until the polyvinyl alcohol was completely dissolved. The temperature was set to 80 ° C, 3,4-dihydroxybenzaldehyde (0.04 g, 0.29 mmol) was added, and dilute hydrochloric acid (1 M) was added, and the reaction was stirred overnight. The solution was cooled to room temperature, poured into a mold, and dried in an oven at 35 ° C to evaporate the solvent to form a film.

[0057] Comparative Example 3

[0058] Preparation of PVA / GTMAC / DBA: w =97000 (2g, 0.02mmol) was added to a round-bottom flask with 40mL of deionized water, and stirred at 90℃ for 2h until the polyvinyl alcohol was completely dissolved. The temperature was set to 80℃, and 10mL of deionized water dissolved glycidyl trimethylammonium chloride (1.72g, 11.3mmol) was added, and 5% sodium hydroxide solution was added and heated and stirred for 3h. Dilute hydrochloric acid (1M) was added to terminate the reaction. The reaction temperature was adjusted to 70℃, and 3,4-dihydroxybenzaldehyde (0.04g, 0.29mmol) was added, and dilute hydrochloric acid (1M) was added, and the reaction was stirred overnight. The solution was cooled to room temperature, poured into a mold, and dried in an oven at 35℃, and the solvent evaporated to form a film.

[0059] In order to verify the existence of intermolecular interactions between PVA and other molecules, FTIR was used between the polymer and the filler. Figure 2 The FTIR spectra of five substances, PVA, PVA / GTMAC, PVA / DBA, PVA / GTMAC / DBA, and PVA / GT MAC / PDA / DBA, are shown. The five substances have a wavelength of 4000-3000 cm -1 The range shows a broad hydroxyl stretching vibration absorption peak, 1717cm -1 The bending vibration of hydroxyl group is 2924cm -1 The asymmetric and symmetric stretching modes of the -CH2- group are attributed to 1422 and 1322 cm -1It is worth noting that after adding other components to PVA, the peak value of the hydroxyl stretching vibration peak increases, and the peak value of the OH stretching vibration increases from 3268cm in the PVA film to -1 Moved to 3342 cm in PVA / GTMAC / PDA / DBA membrane -1 The blue shift means that the hydroxyl groups in DBA and PDA weaken the hydrogen bonds between PVA chains by forming new hydrogen bonds between the catechol structure and the PVA chain. At the same time, the weak broad peak in this peak range gradually turns into a strong broad peak, which is due to the increasing number of hydroxyl groups during the reaction. In the PVA / GTMAC / PDA / DBA spectrum, 1483cm -1 The peak at 1046 cm-1 is attributed to the CH bending of the trimethylammonium group, further indicating successful quaternization. Although the signal of the newly formed C-C bond may be masked by other C-C bond signals, the peak at 1046 cm-1 is -1 At 1469 cm, a clear shoulder absorption appeared, which was attributed to the symmetrical stretching vibration of the aryl alkyl ether (acetal) (COC) bond, indicating that 3,4-dihydroxybenzaldehyde was successfully grafted onto PVA through the acetal reaction. In order to verify the existence of cation-π interaction between quaternary ammonium salt and benzene ring, the characteristic peak of -N(CH3)3 at 1469 cm was observed on PVA / GTMAC. -1 The characteristic peak of PVA / GTMAC / PDA / DBA quaternary ammonium salt is 1483 cm -1 The wave number increases. The characteristic peak of the carbon-carbon double bond on the benzene ring of PVA / DBA increases from 1444 cm -1 Increased to 1489cm -1 , the wave number increases, and a blue shift occurs. The reason for the increase in wave number (blue shift) may be that the electrons of the carbon-carbon double bond on the benzene ring are transferred to the NC bond and CH bond in the quaternary ammonium salt, resulting in an increase in the electron cloud density of the NC bond and the CH bond, which reduces the polarity of the NC bond and the CH bond, that is, the bond strength is enhanced. The greater the vibration frequency of the chemical bond, the more the absorption peak will move to the high wave number region. Similarly, although the electron cloud density of the carbon-carbon double bond on the benzene ring is reduced, the catechol group connected around the benzene ring is an electron-donating group, which can provide electrons for the benzene ring, so that the electron cloud density of the carbon-carbon double bond on the benzene ring increases, the force constant increases, the chemical bond strength increases, the vibration frequency of the chemical bond increases, and the absorption peak moves to the high wave number region, all of which indicate that there is a cation-π interaction between GTMAC and DBA.

[0060] To further investigate the mechanical properties of the hydrogel films, a series of tensile tests were performed using a universal testing machine. Figure 3(a) shows representative tensile stress-strain curves of hydrogel films with different compositions. Pure PVA hydrogel exhibited high tensile strength (35 MPa) and low elongation at break (230%). The hydrogel film of the PVA composite without PDA nanosheets had low tensile strength (15 MPa) and high elongation at break (750%), while the addition of PDA nanosheets improved both the tensile strength and elongation at break of the PVA hydrogel film. This may be attributed to the mechanical reinforcement of the PDA nanosheets and the cation-π interaction between the quaternary ammonium salt and the benzene ring. The rigid network is established by physically cross-linking PVA through hydrogen bonds between the hydroxyl groups on PVA and the highly polar groups (-OH) on PDA. As can be seen from Figure 3(b), when the composite hydrogel film is stretched, the rigid PVA network breaks and effectively consumes energy, which contributes to the high strength (23 MPa) and high toughness (62 MJ / m 3 ).

[0061] In order to verify the effect of PDA nanosheets on the mechanical properties of the hydrogel film, different volumes of PDA nanosheet aqueous solution were added and uniaxial stretching was performed using a universal testing machine. As shown in Figure 4 (a), with the increase of PDA nanosheets, the tensile strength increased significantly, and the elongation at break remained almost unchanged, while at a higher value. However, with the further increase of the PDA nanosheet content, the tensile strength decreased, indicating that PDA nanosheets would change the mechanical properties of the hydrogel film, which may be attributed to the excessive accumulation of PDA nanosheets. According to the tensile stress-strain curve, the PVA composite hydrogel film also showed a tensile strength of 24MPa and an elongation at break of 500%, as well as a high tensile strength of 58MJ / m 3 The ultrahigh toughness can be attributed to the various interactions among the several components of the PVA composite hydrogel film.

[0062] In addition to the cross-linked dry films, wet films cross-linked after immersion in water for 3 days were also tested to simulate the hydration that occurs under physiological conditions. The tensile strength and elongation at break of wet films of PVA composite films with different PDA contents are shown in Figure 4(b). In the cross-linked wet state, the tensile strength and elongation at break of the films were significantly reduced and increased, respectively, compared with the cross-linked dry state; this may be related to the plasticizing effect of the aqueous solution on the PVA composite film. It penetrates into the intersection of the film through the formation of hydrogen bonds between water and PVA and weakens the interaction of adjacent networks, enhancing the flexibility of the polymer structure. In the cross-linked wet state, PDA-12 (PDA addition amount is 12mL) has the best tensile strength (3.1MPa) and elongation at break (520%). This may be due to the addition of PDA, which causes the catechol structure in PDA to form a cation-π interaction with the quaternary ammonium salt, and PDA to form hydrogen bonds with the hydroxyl groups in DBA and PVA. There may also be multiple interactions caused by hydrogen bonds between water and PVA. When the PDA addition amount is less than 12mL, the interaction between adjacent molecules may be weak, resulting in poor mechanical properties. In PDA-16, the PDA content is too high, resulting in the accumulation of PDA, and the interaction process with other molecules is hindered, resulting in poor tensile strength.

[0063] In addition to remarkable mechanical strength, elasticity is also important for prolonging the life of hydrogels and extending their applications. -1The hydrogel was loaded-unloaded at a tensile rate of . Figure 5 (a) At a strain of 50%, the PVA / GTMAC / PDA / DBA wet hydrogel film of Example 1 was further subjected to 10 consecutive loading-unloading cycles to study its fatigue resistance. After 10 consecutive loading-unloading cycles (without rest time), the hysteresis loop of the hydrogel can almost effectively recover to its original value, and the hysteresis loop area of ​​the PVA / GTMAC / PDA / DBA hydrogel film is almost unchanged, probably because the physical network that was broken in each cycle can be immediately restored in the subsequent loading-unloading cycle, indicating that the PVA / GT MAC / PDA / DBA wet hydrogel film has good resilience and fatigue resistance. The good resilience and fatigue resistance of the PVA / GTMAC / PDA / DBA wet hydrogel film are attributed to the effective dissociation-association process of the dynamic cross-linked network. During deformation, the curled polymer chains in the hydrogel become longer. At the same time, the hydrogen bonds and cation-π interactions between the polymer chains dissociate to dissipate energy. After stress release, the deformed network returns to its initial state due to the enhanced elastic contraction of the chain backbone by the cation-π interaction, and then the broken network is effectively restored by reorganizing the cation-π and hydrogen bonds. In Figure 5(b), when the strain increases from 30% to 70%, the hysteresis loop is small, and the stretched hydrogel film can almost return to its original state, indicating that the synthesized hydrogel film has excellent resilience after stretching, which is attributed to the cation-π interaction and hydrogen bonding that promote the formation of PVA domains, resulting in the formation of a dense microporous network structure inside the hydrogel film, indicating that the hydrogel film with interactions between components and PVA domains can effectively dissipate energy when subjected to stress. Good resilience and fatigue resistance ensure the durability and reliability of the tough PVA / GTMAC / PDA / DBA wet hydrogel film.

[0064] After being immersed in water for 3 days, the rectangular PVA hydrogel film increased significantly in size. The real-time swelling curve in the figure shows that the water content of the PVA composite hydrogel film in deionized water remained almost unchanged at about 79wt% within 3 days, and after being immersed in water for 7 days, the size of the sample hardly changed, indicating that the polymer film has good anti-swelling properties.

[0065] The resistance of the PVA composite film was measured using two probes (digital multimeter), and the conductivity was calculated using the formula. It was found that with the increase of PDA content, the conductivity gradually increased, indicating that the nanosheets can improve the conductivity of the system.

[0066] Table 1

[0067] Material Conductivity (S / m) PDA-4 0.0089 PDA-8 0.0145 PDA-12 0.0251 PDA-16 0.0367

[0068] In summary, we have successfully developed a conductive hydrogel film with high strength, high toughness and excellent anti-swelling property through a one-pot method. The densification of polymer chains caused by drying and rehydration leads to the formation of a compact and stable network with multiple cross-linking interactions, including cation-π interactions, crystalline domains and hydrogen bonds between PVA, GTMAC and DBA chains. These interactions greatly improve the mechanical properties and anti-swelling ability of the obtained PVA composite hydrogel film. The anti-swelling high-performance hydrogel has good swelling resistance and high toughness, and has broad application prospects in the fields of tissue repair, brain-computer interface, etc. It can be used in medical dressings, medical devices, biosensors and other fields, which helps to improve the performance and function of materials and promote the development of medical technology.

[0069] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a conductive material with high strength and high toughness and anti-swelling properties, characterized in that: Here are the steps: Step 1: Add glycidyl trimethylammonium chloride aqueous solution and sodium hydroxide aqueous solution to the polyvinyl alcohol aqueous solution, react at 70-90° C. for 2-4 hours, and then add dilute hydrochloric acid to terminate the reaction; Step 2: Add the polydopamine nanosheet aqueous solution to the solution obtained in step 1, and stir the mixture at 60-80° C. for more than 6 hours; Step 3: Add 3,4-dihydroxybenzaldehyde and dilute hydrochloric acid to the solution obtained in step 2, and stir at 60-80° C. for 8-12 hours; Step 4: The solution is cooled to room temperature, poured into a mold, and dried in an oven at 35-45°C to evaporate the solvent and form a film; The molar ratio of the polyvinyl alcohol, glycidyl trimethyl ammonium chloride, polydopamine nanosheets and 3,4-dihydroxybenzaldehyde is 0.02-0.04: 11.3-22.6: 0.48-0.92: 0.29-0.

58.

2. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The polyvinyl alcohol is M w It is 40000~120000 polyvinyl alcohol.

3. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The concentration of the polyvinyl alcohol aqueous solution in step 1 is 0.0005 mol / L to 0.001 mol / L.

4. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The concentration of glycidyl trimethylammonium chloride in step 1 is 1.13 mol / L to 2.26 mol / L.

5. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The amount of dilute hydrochloric acid in step 1 is 0.05 to 0.1 times that of glycidyl trimethylammonium chloride.

6. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The concentration of the polydopamine nanosheet aqueous solution in step 2 is 0.012 mol / L to 0.024 mol / L.

7. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The amount of dilute hydrochloric acid in step 3 is 1.6 to 1.8 times that of 3,4-dihydroxybenzaldehyde.

8. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The concentration of the sodium hydroxide aqueous solution in step 1 is 4wt% to 7wt%.

9. The method for preparing the anti-swelling, high-strength and high-toughness conductive material according to claim 1, characterized in that: The concentration of the dilute hydrochloric acid in step 1 and step 3 is 0.5 mol / L to 1.5 mol / L.

10. The anti-swelling, high-strength and high-toughness conductive material prepared according to the method for preparing the anti-swelling, high-strength and high-toughness conductive material according to any one of claims 1 to 9.