Antibacterial transparent nylon as well as preparation method and application thereof

By preparing antibacterial transparent nylon materials, the problem of deterioration of food packaging materials under the action of light and oxygen is solved, and a solution with high barrier properties and low processing difficulty is provided. It is suitable for bottle filling and realizes the protection against E. coli and Effective inhibition of Staphylococcus aureus.

CN118755261APending Publication Date: 2024-10-11JIANGSU JINGLIHUA NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411119775.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing food packaging materials are prone to deterioration under the action of light and oxygen. The oxygen barrier properties of traditional PET bottles and PE bottles are insufficient and cannot meet the use requirements of modern beverage products. Moreover, the composite film is difficult to process, difficult to recycle, and cannot be applied to Bottle filling.

Method used

Antibacterial transparent nylon material composed of nylon, antibacterial masterbatch, nucleating agent, antioxidant, anti-aging agent and coupling agent is used to prepare the original antibacterial agent powder through a specific grinding, soaking, washing and uniform dispersion process, and is combined with Nylon powder is mixed, and antibacterial masterbatch is prepared through a strip rolling machine. Finally, antibacterial transparent nylon is prepared through high-speed plastic mixing and extrusion granulation process.

Benefits of technology

The prepared antibacterial transparent nylon has good antibacterial, high light transmittance and high barrier properties, is suitable for bottle filling, has low processing difficulty, is easy to recycle, can effectively inhibit E. coli and Staphylococcus aureus, and meets the requirements of food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses antibacterial transparent nylon as well as a preparation method and application thereof in the technical field of high polymer material modification. The antibacterial transparent nylon is prepared from the following raw materials in parts by mass: 100 parts of nylon, 0.1 to 30 parts of antibacterial master batch, 0.01 to 0.5 part of nucleating agent, 0.01 to 0.8 part of antioxidant, 0.01 to 0.8 part of anti-aging agent and 0.01 to 0.8 part of coupling agent. The antibacterial transparent nylon provided by the invention has good inhibition on escherichia coli and staphylococcus aureus, can be used for preparing an antibacterial high-barrier nylon material meeting packaging requirements, is suitable for bottle filling, and is low in processing difficulty and easy to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer material modification, and in particular to an antibacterial transparent nylon and a preparation method and application thereof. Background Art

[0002] Polyamide engineering plastics (PA), also known as nylon, refers to a linear thermoplastic polymer with repeating structural units of amide groups (-CONH) on the main chain. It is obtained by polycondensation of dibasic acid and diamine or amino acid. The amide group of nylon is polar, and hydrogen bonds are formed between molecules, so nylon has excellent properties such as strong wear resistance, impact resistance, fatigue resistance, corrosion resistance, oil resistance, solvent resistance, non-toxicity, good self-extinguishing property, and good electronic insulation. It is mainly used in mechanical instruments, automobiles, textiles, etc. to make bearings, gears, turbines, auto parts, oil pipes, fuel tanks, etc. It is currently one of the most widely used, fastest growing, and most studied types of engineering plastics.

[0003] At present, beverage packaging mostly adopts composite film paper cans, PET (polyethylene terephthalate) bottles, PE (polyethylene) bottles, glass bottles or metal cans. In recent years, with the continuous improvement of residents' living standards, beverage products such as dairy products, dairy beverages, compound fruit juices and fruit and vegetable juices have developed rapidly. However, such beverage products are very easy to deteriorate under the influence of light, oxygen and other factors during the shelf life, resulting in loss of taste or efficacy. The oxygen barrier performance of the current film used for food packaging is poor. After the life of the oxygen-absorbing material in it expires, the barrier performance of the packaging material is greatly reduced. Traditional PET bottles and PE bottles can no longer meet their use requirements, and more expensive glass bottles or metal cans are needed for packaging. This type of composite filling bottle has the characteristics of high recycling cost and poor resistance to falling.

[0004] Patent CN202023024176.0 provides an antibacterial and anti-fog barrier film for frozen food packaging, which is composed of an antibacterial polyamide layer, a first puncture-resistant polyamide layer, an EVOH barrier layer, a second puncture-resistant polyamide layer and a polyamide heat-sealing layer from the outside to the inside; Patent CN202320217753.2 provides an easy-to-tear composite film for freeze-dried fruit tea packaging bags, and its core essence is still a multi-layer composite film. The films involved in the appeal patents are all multi-layer composite materials. This type of film has high processing difficulty and puts forward higher requirements on equipment. Since the film is a composite film, the composite between different materials ultimately increases the difficulty of recycling, and the above-mentioned films are all flat packaging films and cannot be used for bottle filling. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an antibacterial transparent nylon and a preparation method and use thereof. The antibacterial transparent nylon has the characteristics of antibacterial, high transparency, high barrier, etc., and can be used in food packaging, especially suitable for bottle filling.

[0006] To achieve the above object, the present invention is implemented by adopting the following technical solutions:

[0007] In a first aspect, the present invention provides an antibacterial transparent nylon, which is made of the following raw materials in parts by weight: 100 parts of nylon, 0.1 to 30 parts of antibacterial masterbatch, 0.01 to 0.5 parts of nucleating agent, 0.01 to 0.8 parts of antioxidant, 0.01 to 0.8 parts of anti-aging agent, and 0.01 to 0.8 parts of coupling agent.

[0008] Furthermore, the nylon is selected from one or more of nylon 66, nylon 56, nylon 516, MXD6, PACM12 and PA 6T / 6I.

[0009] Further, the nucleating agent is selected from one or more of an inorganic nucleating agent and an organic nucleating agent;

[0010] Wherein, the inorganic nucleating agent is selected from one or more of talc, silica, calcium carbonate and mica powder, wherein the mesh size of talc, silica, calcium carbonate and mica powder is 200 mesh to 4000 mesh; the inorganic nucleating agent is selected from one or more of sorbitol and its derivatives and aromatic phosphate salt nucleating agents.

[0011] Further, the antioxidant is selected from one or more of hindered phenol antioxidants, phosphite antioxidants, amine antioxidants and thioester antioxidants;

[0012] Among them, the hindered phenol antioxidant is selected from one or more of antioxidant 1098, antioxidant 1010 and antioxidant 1024; the phosphite antioxidant is selected from one or more of antioxidant 168, antioxidant 618 and antioxidant 9928; the amine antioxidant is selected from one or more of antioxidant 5057 and antioxidant FS042; the thioester antioxidant is selected from one or more of antioxidant 412S and DLTDP.

[0013] Furthermore, the coupling agent is selected from one or more of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent.

[0014] Furthermore, the antibacterial agent is prepared by a method comprising the following steps:

[0015] The natural zeolite is ground into nanometer scale, and then soaked in hydrochloric acid to obtain the soaked zeolite;

[0016] The soaked zeolite is repeatedly washed with deionized water and centrifuged until the washed water is neutral, thereby obtaining washed zeolite;

[0017] The washed zeolite is added into water and dispersed evenly, then silver nitrate is added and stirred thoroughly, and then ferrous sulfate solution is added to fully reduce the silver nitrate to obtain a solid after the reaction;

[0018] The solid after the reaction is fully washed with dilute hydrochloric acid until no iron ions remain in the zeolite, and finally the zeolite is washed with deionized water until it is neutral to obtain the original powder of the antibacterial agent;

[0019] The antibacterial agent raw powder and nylon powder are mixed evenly, and then a binder is added and mixed evenly, and then the antibacterial masterbatch is prepared through a rolling machine.

[0020] Furthermore, the antibacterial masterbatch is prepared by a method comprising the following steps:

[0021] The natural zeolite is ground into nanometer scale, and then soaked in 30-40wt% concentrated hydrochloric acid for 22-26h to obtain the soaked zeolite;

[0022] The soaked zeolite is repeatedly washed with deionized water and centrifuged until the washed water is neutral, thereby obtaining washed zeolite;

[0023] The washed zeolite is added into water and dispersed evenly, the proportion of zeolite is 1-50wt%t of water, then silver nitrate is added and stirred thoroughly, the proportion of silver nitrate is 0.01-2wt% of zeolite, and then sodium pyrosulfate solution is added to fully reduce the silver nitrate to obtain a solid after reaction;

[0024] The solid after the reaction is fully washed with dilute hydrochloric acid until no iron ions remain in the zeolite, and finally the zeolite is washed with deionized water until it is neutral to obtain the original powder of the antibacterial agent;

[0025] The antibacterial agent raw powder and nylon powder are evenly mixed in a mass ratio of 1:100-1:1000, 0.1-3wt% of a binder is added and mixed evenly, and an antibacterial masterbatch is prepared by a rolling mill.

[0026] In a second aspect, the present invention provides a method for preparing the antibacterial transparent nylon, comprising:

[0027] Obtain raw materials by weight and mix them thoroughly;

[0028] The fully mixed raw materials are extruded and granulated to obtain antibacterial transparent nylon.

[0029] Furthermore, the fully mixing is carried out by using a plastic high-speed mixer, and the process conditions are stirring for 10 to 20 min at a speed of 600 r / min to 800 r / min and a temperature of 0 to 30° C.;

[0030] And / or, the extrusion granulation uses a twin-screw extruder or a single-screw extruder.

[0031] In a third aspect, the present invention provides use of the antibacterial transparent nylon or the antibacterial transparent nylon prepared by the preparation method in food packaging.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The antibacterial transparent nylon provided by the present invention comprises the following raw materials in parts by weight: 100 parts of nylon, 0.1-30 parts of antibacterial masterbatch, 0.01-0.5 parts of nucleating agent, 0.01-0.8 parts of antioxidant, 0.01-0.8 parts of anti-aging agent and 0.01-0.8 parts of coupling agent. The antibacterial transparent nylon provided by the present invention has good inhibition on Escherichia coli and Staphylococcus aureus, can be used to prepare antibacterial high-barrier nylon material meeting packaging requirements, is suitable for bottle filling, has low processing difficulty and is easy to recycle. DETAILED DESCRIPTION

[0034] The present invention is further described below. The following examples are only used to more clearly illustrate the technical solution of the present invention, and are not intended to limit the protection scope of the present invention.

[0035] The preparation method of the antibacterial masterbatch used in the embodiment of the present invention is:

[0036] Weigh 1 kg of natural zeolite and grind it to nanometer scale. After sieving, add 37%wt concentrated hydrochloric acid until the zeolite is submerged, and soak for 24 hours to obtain treated zeolite.

[0037] The soaked zeolite is repeatedly washed with deionized water and centrifuged until the washed water is neutral, thereby obtaining washed zeolite;

[0038] The treated zeolite is added to water and dispersed evenly, the zeolite accounts for 10%wt of the water, then silver nitrate is added and stirred thoroughly, the silver nitrate accounts for 0.1%wt of the zeolite, and then ferrous sulfate solution is added to fully reduce the silver nitrate to obtain a reacted solid;

[0039] The solid after the reaction is fully washed with dilute hydrochloric acid until no iron ions remain in the zeolite, and finally the zeolite is washed with deionized water until it is neutral to obtain the original powder of the antibacterial agent;

[0040] The antibacterial agent raw powder and nylon powder are mixed evenly, wherein the content of the antibacterial agent raw powder is 10wt% of the total powder, 3wt% of the adhesive is added and mixed evenly, and the antibacterial masterbatch is prepared by a rolling mill.

[0041] Example 1

[0042] The present embodiment provides an antibacterial transparent nylon and a preparation method thereof. The antibacterial transparent nylon is made of the following raw materials in parts by weight: 100 parts of nylon 66, 0.3 parts of sorbitol, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch and 0.2 parts of anti-ultraviolet agent (Tinuvin 329).

[0043] The preparation method of the antibacterial transparent nylon is as follows:

[0044] (1) All raw materials except the antibacterial masterbatch were taken by weight, and stirred in a plastic high-speed mixer at a speed of 1000 r / min and a temperature of 80° C. for 10 minutes to fully mix them;

[0045] (2) Add the mixed material into the hopper of the twin-screw extruder and start the twin-screw extruder.

[0046] (3) The antibacterial masterbatch is added into a twin-screw extruder by side feeding, and is extruded together with the mixed material through the twin-screw extruder to obtain antibacterial transparent nylon.

[0047] Example 2

[0048] The present embodiment provides an antibacterial transparent nylon and a preparation method thereof. The antibacterial transparent nylon is made of the following raw materials in parts by weight: 100 parts of MXD6, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch and 0.2 parts of anti-ultraviolet aging agent.

[0049] The preparation method of the antibacterial transparent nylon is the same as that of Example 1.

[0050] Example 3

[0051] The present embodiment provides an antibacterial transparent nylon and a preparation method thereof. The antibacterial transparent nylon is made of the following raw materials in parts by weight: 100 parts of PACM12, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch, and 0.2 parts of anti-ultraviolet aging agent.

[0052] The preparation method of the antibacterial transparent nylon is the same as that of Example 1.

[0053] Example 4

[0054] The present embodiment provides an antibacterial transparent nylon and a preparation method thereof. The antibacterial transparent nylon is made of the following raw materials in parts by weight: 100 parts of PA 6T / 6I, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch, and 0.2 parts of anti-ultraviolet aging agent.

[0055] The preparation method of the antibacterial transparent nylon is the same as that of Example 1.

[0056] Example 5

[0057] The present embodiment provides an antibacterial transparent nylon and a preparation method thereof. The antibacterial transparent nylon is made of the following raw materials in parts by weight: 100 parts of PA6, 0.3 parts of nucleating agent TMP-5, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch, and 0.2 parts of anti-ultraviolet aging agent.

[0058] The preparation method of the antibacterial transparent nylon is the same as that of Example 1.

[0059] Comparative Example 1

[0060] This comparative example provides a nylon and a preparation method thereof, which are made of the following raw materials in parts by mass: 100 parts of PA6, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, 1 part of antibacterial masterbatch, and 0.2 parts of anti-ultraviolet aging agent.

[0061] The preparation method is the same as that in Example 1.

[0062] Comparative Example 2

[0063] This comparative example provides a nylon and a preparation method thereof, which are made from the following raw materials in parts by mass: 100 parts of PA66, 0.3 parts of sorbitol, 0.1 parts of antioxidant 1098, 0.1 parts of antioxidant 168, and 0.2 parts of an anti-ultraviolet aging agent.

[0064] The preparation method is the same as that in Example 1.

[0065] The nylon provided in Examples 1 to 5 and Comparative Examples 1 and 2 were put into a bottle making machine for production to obtain transparent nylon plastic bottles, and the antibacterial effect, haze and oxygen permeability were tested respectively.

[0066] The test method for antibacterial samples refers to GB / T2591-2003A "Test methods and antibacterial effects of antibacterial plastics";

[0067] The test method of Fog City refers to ASTMD1003-97 "Fog and light transmittance of transparent plastics";

[0068] The oxygen transmission rate test method refers to ASTM F1927 "Standard Test Method for Determining Oxygen Transmission Rate, Permeability, and Permeability Through Barrier Materials Using a Coulometric Detector".

[0069] The test results are shown in the following table.

[0070] Table 1 Test results of antibacterial effect, haze and oxygen transmission rate

[0071]

[0072] It can be seen from the above data that the examples (Examples 1 to 5 and Comparative Example 1) with the addition of antibacterial masterbatch have good inhibitory properties against Escherichia coli and Staphylococcus aureus, while the example (Comparative Example 2) without the addition has no inhibitory effect.

[0073] By comparing Comparative Example 1 with Example 1, it can be seen that after adding the nucleating agent, the light transmittance of the material is greatly improved, which is more conducive to being used in food packaging.

[0074] The embodiments of the present invention are described above, but the present invention is not limited to the above-mentioned specific implementation modes. The above-mentioned specific implementation modes are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the purpose of the present invention and the claims, which are all within the protection of the present invention.

Claims

1. An antibacterial transparent nylon, characterized in that: The invention is made of the following raw materials in parts by weight: 100 parts of nylon, 0.1 to 30 parts of antibacterial masterbatch, 0.01 to 0.5 parts of nucleating agent, 0.01 to 0.8 parts of antioxidant, 0.01 to 0.8 parts of anti-aging agent and 0.01 to 0.8 parts of coupling agent.

2. The antibacterial transparent nylon according to claim 1, characterized in that: The nylon is selected from one or more of nylon 66, nylon 56, nylon 516, MXD6, PACM12 and PA 6T / 6I.

3. The antibacterial transparent nylon according to claim 1, characterized in that: The nucleating agent is selected from one or more of an inorganic nucleating agent and an organic nucleating agent; Wherein, the inorganic nucleating agent is selected from one or more of talc, silica, calcium carbonate and mica powder, wherein the mesh size of talc, silica, calcium carbonate and mica powder is 200 mesh to 4000 mesh; the inorganic nucleating agent is selected from one or more of sorbitol and its derivatives and aromatic phosphate salt nucleating agents.

4. The antibacterial transparent nylon according to claim 1, characterized in that: The antioxidant is selected from one or more of hindered phenol antioxidants, phosphite antioxidants, amine antioxidants and thioester antioxidants; Among them, the hindered phenol antioxidant is selected from one or more of antioxidant 1098, antioxidant 1010 and antioxidant 1024; the phosphite antioxidant is selected from one or more of antioxidant 168, antioxidant 618 and antioxidant 9928; the amine antioxidant is selected from one or more of antioxidant 5057 and antioxidant FS042; the thioester antioxidant is selected from one or more of antioxidant 412S and DLTDP.

5. The antibacterial transparent nylon according to claim 1, characterized in that: The coupling agent is selected from one or more of a silane coupling agent, a titanate coupling agent and an aluminate coupling agent.

6. The antibacterial transparent nylon according to claim 1, characterized in that: The antibacterial agent is prepared by a method comprising the following steps: The natural zeolite is ground into nanometer scale, and then soaked in hydrochloric acid to obtain the soaked zeolite; The soaked zeolite is repeatedly washed with deionized water and centrifuged until the washed water is neutral, thereby obtaining washed zeolite; The washed zeolite is added into water and dispersed evenly, then silver nitrate is added and stirred thoroughly, and then ferrous sulfate solution is added to fully reduce the silver nitrate to obtain a solid after the reaction; The solid after the reaction is fully washed with dilute hydrochloric acid until no iron ions remain in the zeolite, and finally the zeolite is washed with deionized water until it is neutral to obtain the original powder of the antibacterial agent; The antibacterial agent raw powder and nylon powder are mixed evenly, and then a binder is added and mixed evenly, and then the antibacterial masterbatch is prepared through a rolling machine.

7. The antibacterial transparent nylon according to claim 6, characterized in that: The antibacterial masterbatch is prepared by a method comprising the following steps: The natural zeolite is ground into nanometer scale, and then soaked in 30-40wt% concentrated hydrochloric acid for 22-26h to obtain the soaked zeolite; The soaked zeolite is repeatedly washed with deionized water and centrifuged until the washed water is neutral, thereby obtaining washed zeolite; The washed zeolite is added into water and dispersed evenly, the proportion of zeolite is 1-50wt%t of water, then silver nitrate is added and stirred thoroughly, the proportion of silver nitrate is 0.01-2wt% of zeolite, and then sodium pyrosulfate solution is added to fully reduce the silver nitrate to obtain a solid after reaction; The solid after the reaction is fully washed with dilute hydrochloric acid until no iron ions remain in the zeolite, and finally the zeolite is washed with deionized water until it is neutral to obtain the original powder of the antibacterial agent; The antibacterial agent raw powder and nylon powder are evenly mixed in a mass ratio of 1:100-1:1000, 0.1-3wt% of a binder is added and mixed evenly, and an antibacterial masterbatch is prepared by a rolling mill.

8. A method for preparing the antibacterial transparent nylon according to any one of claims 1 to 7, characterized in that: include: Obtain raw materials by weight and mix them thoroughly; The fully mixed raw materials are extruded and granulated to obtain antibacterial transparent nylon.

9. The method for preparing antibacterial transparent nylon according to claim 8, characterized in that: The fully mixing is carried out by using a plastic high-speed mixer, and the process conditions are: stirring for 10 to 20 minutes at a speed of 600 r / min to 800 r / min and a temperature of 0 to 30°C; And / or, the extrusion granulation uses a twin-screw extruder or a single-screw extruder.

10. Use of the antibacterial transparent nylon according to any one of claims 1 to 7 or the antibacterial transparent nylon prepared by the preparation method according to claim 8 or 9 in food packaging.

Citation Information

Cited By

  • Food packaging film easy to tear linearly and preparation process thereof

    CN119331410A