Passivating agent for photovoltaic cell as well as preparation method and application of passivating agent

By using a passivator of polyimide resin and fluororesin containing active groups, combined with a protective film of fluororesin and polyvinylidene fluoride, the problem of efficiency loss after cutting of photovoltaic cells in the existing technology is solved and achieved More efficient passivation effect and improved component performance.

CN118755320APending Publication Date: 2024-10-11DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410797375.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing photovoltaic cell passivation liquid cannot effectively reduce the cutting loss of the cells and increase the module power after laser cutting, and the passivation effect is poor.

Method used

A passivator composed of polyimide resin and fluororesin containing active groups is used to form a stable covalent bond through the reaction of the active groups with the cut surface of the cell, combining the dielectric properties of the fluororesin and the polyvinylidene fluoride Ethylene protective film significantly improves passivation effect.

Benefits of technology

It significantly reduces the efficiency loss of small pieces after cell cutting, increases module power, reduces the cost per watt, and provides a longer-lasting passivation effect and improved electrical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755320A_ABST
    Figure CN118755320A_ABST
Patent Text Reader

Abstract

The invention provides a passivator for a photovoltaic cell as well as a preparation method and application of the passivator, and relates to the technical field of photovoltaic cells, the passivator for the photovoltaic cell comprises the following components in percentage by mass: 5-8% of polyimide resin containing active groups, 5-8% of fluororesin and the balance of solvent; wherein the active group comprises at least one of amino and hydroxyl. The active group-containing polyimide resin is easy to form a film on a semiconductor and has better passivation performance, and the fluororesin and the active group-containing polyimide resin act together to passivate the cut surface of the battery piece, so that the cutting loss of the battery piece is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic cells, and in particular to a passivating agent for photovoltaic cells, a preparation method thereof and an application thereof. Background Art

[0002] With the continuous development of photovoltaic cell and module technology, competition in the photovoltaic field is becoming increasingly fierce. Improving module power and reducing costs have become important tasks in this field. The current module manufacturing technology is to use a laser scriber to cut the entire cell into two equal halves or more equal slices to reduce the internal circuit and internal friction of the module. However, when using laser to cut the cell, the high temperature melting of the laser destroys the cell structure and impurity contamination, resulting in partial efficiency loss of the cell. The method currently used usually uses a passivation solution for passivation treatment, using the effective ingredients in the passivation solution to passivate the cut surface of the cell and reduce the surface recombination center, so as to achieve the purpose of reducing the efficiency loss of the cell and increasing the power of the module.

[0003] The existing passivation solution is usually a single-component passivation solution containing monomers such as ozone and polyimide, which has a poor passivation effect on the cut battery cells and cannot further reduce the cutting loss of the battery cells.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a passivator for photovoltaic cells, which comprises the following components by mass percentage: 5%-8% of polyimide resin containing active groups, 5%-8% of fluororesin and the remainder of solvent; wherein the active groups include at least one of amino and hydroxyl groups. The polyimide resin containing active groups is easy to form a film on a semiconductor and has better passivation performance, and the fluororesin and the polyimide resin containing active groups work together to passivate the cut surface of the cell, further reducing the cell cutting loss.

[0006] The second object of the present invention is to provide a method for preparing a passivator for photovoltaic cells. In the preparation method, a polyimide resin containing active groups and a fluororesin are dissolved in a solvent, and the passivator prepared by the preparation method has a better passivation effect.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] In a first aspect, the present invention provides a passivator for photovoltaic cells, the passivator comprising the following components by mass percentage: 5%-8% of a polyimide resin containing an active group, 5%-8% of a fluororesin and the remainder of a solvent;

[0009] Wherein, the active group includes at least one of an amino group and a hydroxyl group.

[0010] Taking the total mass of the passivator as 100%, the added amount of the polyimide resin containing active groups is 5%-8%, for example, but not limited to 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, or 8%.

[0011] Based on the total mass of the passivator as 100%, the added amount of the fluororesin is 5%-8%, for example, but not limited to 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, or 8%.

[0012] In the present invention, polyimide has excellent passivation performance and electrical insulation, and active groups are added to the polyimide resin on its basis, and the active groups are attached to the polyimide resin groups to form polymers. The added active groups include organic groups such as amino (-NH2) and hydroxyl (-OH), and both of these groups have an exposed molecular bond or ionic bond, which have strong activity and can combine with free molecules or ionic bonds to form stable covalent bonds. In the cut surface of the battery cell, there are a large number of free Si-H bonds, and the active groups react and combine with them to form Si-NH bonds and CO-Si bonds, which avoids the combination of impurity molecules or ions with Si-H bonds to destroy the dielectric stability of the cut surface, and further enhances the passivation effect.

[0013] Preferably, the fluororesin includes at least one of polyvinylidene fluoride, polytetrafluoroethylene and polychlorotrifluoroethylene, and the solvent includes at least one of an alcohol solvent and water;

[0014] Preferably, the alcohol solvent includes at least one of methanol, ethanol and propanol;

[0015] Preferably, the water comprises clean water that has been filtered and sterilized.

[0016] Preferably, the photovoltaic cell passivator comprises the following components by mass percentage: 5%-8% of polyimide resin containing active groups, 5%-8% of fluororesin, 3%-5% of ethanol and the balance of water.

[0017] Taking the total mass of the passivator as 100%, the added amount of the polyimide resin containing active groups is 5%-8%, for example, but not limited to 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, or 8%.

[0018] Based on the total mass of the passivator as 100%, the added amount of the fluororesin is 5%-8%, for example, but not limited to 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, or 8%.

[0019] Taking the total mass of the passivator as 100%, the added amount of ethanol is 3%-5%, for example, but not limited to 3%, 3.5%, 4%, 4.5% or 5%.

[0020] In the present invention, the fluororesin is polyvinylidene fluoride, which has a passivation property due to its own dielectric properties, and can passivate the cut surface of the cell, and work together with polyimide to passivate the cut surface of the cell. At the same time, polyvinylidene fluoride has excellent properties such as anti-aging, acid and alkali resistance, weather resistance, and ultraviolet radiation resistance, and can form a protective film after the subsequent cell is made into a component, which can ensure the passivation effect of the cut surface of the cell and the power generation effect itself for a longer time; ethanol mainly plays the role of dispersing organic matter, so that the polyimide resin, polyvinylidene fluoride and active groups can be evenly dispersed and easily dissolved in the water solvent.

[0021] In the present invention, polyimide and polyvinylidene fluoride passivate the composite surface formed by cutting the battery cell to repair surface defects. The polyimide and polyvinylidene fluoride layers carry a certain amount of negative charge, which significantly reduces the positive charge of the surface layer of the battery cell cut, and plays a passivation role; in addition, the surface is purified after passivation, reducing pollution, thereby improving the electrical properties of the cut surface; the active groups react with the Si-H dangling bonds on the cut surface, so that the surface defects and free Si-H dangling bonds no longer become the recombination centers of electrons and holes, and the cut surface is double passivated; the above three work together to repair the defects of the battery cut surface, and have an excellent passivation effect, and polyvinylidene fluoride forms a physical protective film after drying to avoid contamination by impurities and the occurrence of other reactions, thereby reducing the loss of efficiency after the battery cell is cut, improving the power of the battery cell assembly and ensuring the passivation effect and assembly performance.

[0022] In a second aspect, the present invention provides a method for preparing the photovoltaic cell passivator, the preparation method comprising the following steps:

[0023] The polyimide resin and fluororesin containing active groups in a prescribed amount are dissolved in a solvent to obtain a passivating agent.

[0024] Preferably, the polyimide resin containing active groups and the fluororesin in the formulated amount are dissolved in ethanol to obtain a mixture, and then the mixture is dissolved in water to obtain a passivating agent;

[0025] Preferably, the mixture is dissolved in the solvent step at a temperature of 250-280°C, for example, but not limited to 250°C, 255°C, 260°C, 265°C, 270°C, 275°C or 280°C, and a pressure of 3Mpa-3.3Mpa, for example, but not limited to 3Mpa, 3.1Mpa, 3.2Mpa or 3.3Mpa.

[0026] Preferably, the polyimide resin containing active groups is prepared by the following steps:

[0027] The polyimide resin is mixed with an acetone solution, and then 1,3-diaminoguanidine hydrochloride and ethylene glycol are added, and the mixture is mixed under a nitrogen atmosphere to obtain a polyimide resin containing an active group;

[0028] Preferably, the molar ratio of 1,3-diaminoguanidine hydrochloride to ethylene glycol is 1:1; in the stirring step, the temperature is 200-250°C, for example, it can be, but not limited to 200°C, 210°C, 220°C, 230°C, 240°C or 250°C, and the stirring time is 10-12h, for example, it can be, but not limited to 10h, 11h or 12h.

[0029] In the present invention, the polymer of the active group and the polyimide resin is prepared by an organic polymerization reaction. Preferably, the polyimide resin is prepared by the following steps:

[0030] The dianhydride and the diamine react to obtain polyamic acid, the polyamic acid is dehydrated and cyclized to obtain polyisoimide, and the polyisoimide is isomerized to obtain polyimide resin.

[0031] In the present invention, dianhydride and diamine are reacted to obtain polyamic acid, which is then dehydrated and cyclized to polyisoimide under the action of a dehydrating agent, and is finally isomerized to polyimide resin under the action of a catalyst or under heat treatment conditions.

[0032] Preferably, the molar ratio of the dianhydride to the diamine is (0.8-0.9):1, for example, it may be, but is not limited to, 0.8:1, 0.85:1 or 0.9:1.

[0033] Preferably, the dehydrating agent comprises at least one of propanol, n-butanol and tert-butanol;

[0034] Preferably, the catalyst comprises at least one of an organic acid and an organic base;

[0035] Preferably, the organic acid comprises at least one of acetic acid and benzoic acid;

[0036] Preferably, the organic base comprises at least one of potassium ethoxide and pyridine;

[0037] Preferably, the heat treatment temperature is 100-250°C, for example, but not limited to 100°C, 150°C, 200°C or 250°C.

[0038] In the present invention, the reaction is carried out under the conditions of organic acid or organic base or heat treatment, which can promote the occurrence of the reaction and accelerate the reaction process, and at the same time can make the polyimide resin film-formed with better heat resistance.

[0039] Preferably, the fluororesin comprises polyvinylidene fluoride, and the polyvinylidene fluoride is prepared by polymerizing 1,1-difluoroethylene monomer;

[0040] Preferably, the polymerization temperature is 200-250°C, for example, but not limited to 200°C, 210°C, 220°C, 230°C, 240°C or 250°C, and the pressure is 2-2.5Mpa, for example, but not limited to 2Mpa, 2.1Mpa, 2.2Mpa, 2.3Mpa, 2.4Mpa or 2.5Mpa.

[0041] Furthermore, the method for preparing the passivating agent for photovoltaic cells comprises the following steps:

[0042] Preparation of polyimide resin: mixing dianhydride and diamine in a molar ratio of 0.8-0.9:1, reacting to obtain polyamic acid, adding a dehydrating agent, dehydrating and cyclizing the polyamic acid to obtain polyisoimide, adding an organic acid catalyst or an organic base catalyst or performing heat treatment, isomerizing the polyisoimide to obtain polyimide resin, wherein the heat treatment temperature is 100-250° C.;

[0043] Preparation of a polyimide resin containing active groups: adding a polyimide resin to an acetone solution, then adding 1,3-diaminoguanidine hydrochloride and ethylene glycol in a molar ratio of 1:1, and introducing nitrogen protection, mixing at a temperature of 200° C. to 250° C. for 10 to 12 hours, preferably by stirring, to finally obtain a uniform polyimide resin polymer solution containing amino and hydroxyl groups;

[0044] The temperature is more preferably 200°C, and the stirring time is more preferably 12h.

[0045] Preparation of polyvinylidene fluoride: It is prepared by polymerization of 1,1-difluoroethylene monomer at 200℃-250℃ and 2Mpa-2.5Mpa;

[0046] Among them, the temperature is further preferably 200°C, and the pressure is further preferably 2Mpa;

[0047] Preparation of a passivator for photovoltaic cells: first dissolving a polyimide resin containing an active group and polyvinylidene fluoride in ethanol, then dissolving in water at 250°C-280°C, 3Mpa-3.3Mpa, under constant temperature and pressure, with continuous stirring, and cooling to room temperature to obtain the passivator for photovoltaic cells;

[0048] Among them, calculated by mass percentage, the polyimide resin containing active groups is 5%-8%, the fluororesin is 5%-8%, the ethanol is 3%-5%, and the solvent is 79%-87%. The temperature is further preferably 250° C., and the pressure is further preferably 3Mpa.

[0049] In a third aspect, the present invention provides a use of the photovoltaic cell passivator in passivating a cell.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] The photovoltaic cell passivator provided by the present invention has a main component of a polyimide resin containing an active group, a fluororesin and ethanol, and a main active substance of the polyimide resin containing an active group and polyvinylidene fluoride. The polyimide resin containing an active group is easier to form a film on a semiconductor and has better passivation performance. The fluororesin and the polyimide work together to repair the defects of the cell cutting surface, and have an excellent passivation effect, so that the efficiency loss of the cell chip is reduced, thereby reducing the power loss of the component and reducing the unit watt cost of the component. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0053] Figure 1 The molecular structure diagram of polyimide resin and polyvinylidene fluoride containing active groups;

[0054] Figure 2 Schematic diagram of the passivation principle of polyimide resin and polyvinylidene fluoride containing active groups. DETAILED DESCRIPTION

[0055] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0056] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0058] Example 1

[0059] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 5% of polyimide resin containing active groups, 8% of polyvinylidene fluoride, 3% of ethanol, and 84% of water.

[0060] The photovoltaic cell passivator is prepared by the following steps:

[0061] (a) mixing dianhydride and diamine in a molar ratio of 0.9:1, reacting to obtain polyamic acid, adding a dehydrating agent, dehydrating and cyclizing the polyamic acid to obtain polyisoimide, adding an organic acid catalyst acetic acid for treatment, and isomerizing the polyisoimide to obtain a polyimide resin; wherein the dehydrating agent may be one of propanol, n-butanol and tert-butanol.

[0062] (b) adding a polyimide resin to an acetone solution, and then adding 1,3-diaminoguanidine hydrochloride and ethylene glycol in a molar ratio of 1:1, and introducing nitrogen protection, stirring continuously at a temperature of 200° C. for 12 hours, and finally obtaining a uniform polyimide resin polymer solution containing amino and hydroxyl groups.

[0063] (c) Polyvinylidene fluoride is prepared by polymerization of 1,1-difluoroethylene monomer at 200°C and 2 MPa.

[0064] (d) Dissolving the polyimide resin containing active groups and polyvinylidene fluoride in ethanol according to the above ratio, and then dissolving them in clean water after filtration and sterilization under the conditions of 250° C., 3 MPa, constant temperature and pressure, and continuous stirring, and cooling to room temperature to obtain the passivating agent for photovoltaic cells. The filtration is carried out by microfiltration or ultrafiltration to remove impurities and particles in the water.

[0065] Example 2

[0066] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 8% of polyimide resin containing active groups, 5% of polyvinylidene fluoride, 5% of ethanol, and 82% of water.

[0067] The preparation steps of the photovoltaic cell passivator are consistent with those in Example 1.

[0068] Example 3

[0069] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 84% of water.

[0070] The preparation steps of the photovoltaic cell passivator are consistent with those in Example 1.

[0071] Example 4

[0072] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 84% of water.

[0073] In the preparation step (a) of the photovoltaic cell passivator, the molar ratio of dianhydride to diamine is 0.8:1, and the other preparation steps are consistent with Example 3.

[0074] Example 5

[0075] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 84% of water.

[0076] In the preparation step (a) of the photovoltaic cell passivator, an organic base catalyst pyridine is used, and the other preparation steps are consistent with Example 3.

[0077] Example 6

[0078] The present embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 84% of water.

[0079] In the preparation step (a) of the photovoltaic cell passivator, heat treatment is used instead of adding a catalyst, the temperature of the heat treatment is 100 to 250° C., and the other preparation steps are consistent with Example 3.

[0080] Example 7

[0081] This embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 5% of polyimide resin containing active groups, 8% of polyvinylidene fluoride, and 88% of water.

[0082] In the preparation step (d) of the photovoltaic cell passivator, the polyimide resin containing active groups and polyvinylidene fluoride are dissolved in water, and the other preparation steps are consistent with those in Example 1.

[0083] Example 8

[0084] This embodiment provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 8% of polyimide resin containing active groups, 5% of polyvinylidene fluoride, and 88% of ethanol.

[0085] In the preparation step (d) of the photovoltaic cell passivator, the polyimide resin containing active groups and polyvinylidene fluoride are dissolved in ethanol, and the other preparation steps are consistent with those in Example 2.

[0086] Examples 9-16

[0087] The photovoltaic cell passivators in Examples 1-6 were sprayed on several small cell sheets cut by laser to obtain the passivated cell sheets in Examples 7-12.

[0088] Comparative Example 1

[0089] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide, 6% of polyvinylidene fluoride, 4% of ethanol, and 84% of water.

[0090] In the preparation step (a) of the passivator, the polyisoimide is not subjected to isomerization treatment, and step (b) is not performed. The other preparation steps are consistent with those in Example 3.

[0091] Comparative Example 2

[0092] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% polyimide resin, 6% polyvinylidene fluoride, 4% ethanol, and 84% water.

[0093] In the preparation steps of the passivating agent, step (b) is not performed, and the other preparation steps are consistent with those in Example 3.

[0094] Comparative Example 3

[0095] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 4% of ethanol, and 90% of water.

[0096] In the preparation steps of the passivating agent, step (c) is not performed, and the other preparation steps are consistent with those in Example 3.

[0097] Comparative Example 4

[0098] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% polyvinylidene fluoride, 4% ethanol, and 90% water.

[0099] In the preparation steps of the passivator, steps (a) and (b) are not performed, and the other preparation steps are consistent with Example 3.

[0100] Comparative Example 5

[0101] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 10% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 80% of water.

[0102] The preparation steps of the photovoltaic cell passivator are consistent with those of Example 3.

[0103] Comparative Example 6

[0104] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 1% of polyimide resin containing active groups, 6% of polyvinylidene fluoride, 4% of ethanol, and 89% of water.

[0105] The preparation steps of the photovoltaic cell passivator are consistent with those of Example 3.

[0106] Comparative Example 7

[0107] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 10% of polyvinylidene fluoride, 4% of ethanol, and 80% of water.

[0108] The preparation steps of the photovoltaic cell passivator are consistent with those of Example 3.

[0109] Comparative Example 8

[0110] This comparative example provides a passivator for photovoltaic cells, which comprises the following components by mass percentage: 6% of polyimide resin containing active groups, 1% of polyvinylidene fluoride, 4% of ethanol, and 89% of water.

[0111] The preparation steps of the photovoltaic cell passivator are consistent with those of Example 3.

[0112] Comparative Examples 9-16

[0113] The photovoltaic cell passivators in Comparative Examples 1-8 were sprayed on several small cell sheets cut by laser respectively to obtain the passivated cell sheets in Comparative Examples 9-16.

[0114] Test Case

[0115] Passivation effect test of passivators for photovoltaic cells

[0116] Test samples: the passivated cells in Examples 9-16 and the passivated cells in Comparative Examples 9-16.

[0117] Test method: Test the efficiency of the cell before cutting and test it again after cutting. Subtract the efficiency before and after cutting, and the difference is the cutting loss of the cell, that is, the loss of cell efficiency during the cutting process. The smaller the loss, the more it can ensure high power of the component and reduce costs. Therefore, the smaller the difference in efficiency before and after cutting, the smaller the cutting loss, and the better the passivation effect. Conversely, the effect is poor or no effect.

[0118] The specific test results are shown in Table 1:

[0119] sample Battery cutting loss (%) Example 9 0.21 Example 10 0.19 Embodiment 11 0.22 Example 12 0.20 Example 13 0.22 Embodiment 14 0.24 Embodiment 15 0.25 Example 16 0.18 Comparative Example 9 0.34 Comparative Example 10 0.33 Comparative Example 11 0.30 Comparative Example 12 0.35 Comparative Example 13 0.31 Comparative Example 14 0.33 Comparative Example 15 0.27 Comparative Example 16 0.29

[0120] As can be seen from the data in Table 1, in Examples 9-16, the passivation solution formula contains a polyimide resin containing an active group, and within a suitable ratio range, the passivation performance is better under the condition that an acid or base is used as a catalyst in the synthesis process. In Comparative Examples 9-16, the polyimide resin containing an active group is not contained or the ratio is very low, and the passivation performance is poor under the condition that there is no acid or base catalysis in the synthesis process.

[0121] In the photovoltaic cell passivator provided by the present invention, Figure 1 and Figure 2 As shown, the polyvinylidene fluoride layer carries a negative charge, thereby reducing the positive charge of the cut surface layer of the cell, playing a passivation role. At the same time, the active groups react with the Si-H dangling bonds on the cut surface, so that surface defects and free Si-H dangling bonds no longer become electron-hole recombination centers, achieving an excellent passivation effect.

[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A passivator for photovoltaic cells, characterized in that: The photovoltaic cell passivator comprises the following components by mass percentage: 5%-8% of polyimide resin containing active groups, 5%-8% of fluororesin and the remainder of solvent; Wherein, the active group includes at least one of an amino group and a hydroxyl group.

2. The photovoltaic cell passivator according to claim 1, characterized in that: The fluororesin includes at least one of polyvinylidene fluoride, polytetrafluoroethylene and polychlorotrifluoroethylene, and the solvent includes at least one of an alcohol solvent and water; Preferably, the alcohol solvent includes at least one of methanol, ethanol and propanol; Preferably, the water comprises clean water that has been filtered and sterilized.

3. The photovoltaic cell passivator according to claim 1, characterized in that: The photovoltaic cell passivator comprises the following components by mass percentage: 5%-8% of polyimide resin containing active groups, 5%-8% of fluororesin, 3%-5% of ethanol and the balance of water.

4. A method for preparing a passivating agent for photovoltaic cells according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: The polyimide resin and fluororesin containing active groups in a prescribed amount are dissolved in a solvent to obtain a passivating agent.

5. The preparation method according to claim 4, characterized in that: Dissolving a formulated amount of polyimide resin containing active groups and fluororesin in ethanol to obtain a mixture, and then dissolving the mixture in water to obtain a passivating agent; Preferably, the mixture is dissolved in the solvent step at a temperature of 250-280° C. and a pressure of 3 MPa-3.3 MPa.

6. The preparation method according to claim 4, characterized in that: The polyimide resin containing active groups is prepared by the following steps: The polyimide resin is mixed with an acetone solution, and then 1,3-diaminoguanidine hydrochloride and ethylene glycol are added, and the mixture is mixed under a nitrogen atmosphere to obtain a polyimide resin containing an active group; Preferably, the molar ratio of 1,3-diaminoguanidine hydrochloride to ethylene glycol is 1:1; Preferably, in the mixing step, the temperature is 200-250° C. and the mixing time is 10-12 h.

7. The preparation method according to claim 6, characterized in that: The polyimide resin is prepared by the following steps: The dianhydride and the diamine react to obtain polyamic acid, which is then dehydrated and cyclized to obtain polyisoimide, and then the polyisoimide is isomerized to obtain polyimide resin.

8. The preparation method according to claim 7, characterized in that: The molar ratio of the dianhydride to the diamine is (0.8-0.9):1; The dehydration cyclization adopts a dehydrating agent for dehydration, and the isomerization adopts a catalyst or a heat treatment method; Preferably, the dehydrating agent comprises at least one of propanol, n-butanol and tert-butanol; Preferably, the catalyst comprises at least one of an organic acid and an organic base; Preferably, the organic acid comprises at least one of acetic acid and benzoic acid; Preferably, the organic base comprises at least one of potassium ethoxide and pyridine; Preferably, the heat treatment temperature is 100-250°C.

9. The preparation method according to claim 7, characterized in that: The fluororesin includes polyvinylidene fluoride, which is prepared by polymerizing 1,1-difluoroethylene monomer; Preferably, the polymerization temperature is 200-250° C. and the pressure is 2-2.5 MPa.

10. Use of the photovoltaic cell passivator according to any one of claims 1 to 3 in passivating a cell.

Citation Information

Patent Citations

  • Fluoridated polyimide film for thin-film solar cells and preparation method thereof

    CN103897393A

  • Low temperature curable polyimide resin and method of preparing the same

    US20120016076A1