Metal corrosion inhibition packaging adhesive film, preparation method, application method and photovoltaic module packaging assembly
By using a metal corrosion-inhibiting encapsulating film in busbarless photovoltaic modules, combined with a thermally cured adhesive layer and a thermoplastic corrosion-inhibiting layer, the problem of shadows under the soldering strips is solved, improving the reliability of the module and reducing costs, achieving It effectively protects active metal materials and reduces PID power attenuation.
Patent Information
- Application Number
- CN202410996055.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-24
AI Technical Summary
During the packaging process of busbarless photovoltaic modules, there is a problem of shadows under the solder ribbons, resulting in insufficient conductive connections and poor module reliability. Existing solutions such as pre-cross-linked EVA, POE film or high-flow PVB film are costly. , which is not conducive to component cost reduction and efficiency improvement.
A metal corrosion-inhibiting encapsulating film is used, including a heat-curing adhesive layer and a thermoplastic corrosion-inhibiting layer. The heat-curing adhesive layer is composed of a cross-linkable matrix resin, a peroxide cross-linking agent, an auxiliary cross-linking agent, a coupling agent and a light-stabilizing layer. Agent composition, thermoplastic The corrosion inhibition layer is composed of thermoplastic matrix resin, plasticizer, coupling agent and corrosion inhibitor. The corrosion inhibitor forms a thermoplastic corrosion inhibition layer with a thickness of 10-200 μm through a slit coating process to prevent oxidative corrosion of active metal materials.
It effectively solves the problem of shadows under the welding ribbon, improves the long-term reliability of the component, reduces the PID power attenuation rate, and costs less than traditional pure thermoplastic PVB film.
Smart Images

Figure BDA0004960238270000021 
Figure BDA0004960238270000022 
Figure BDA0004960238270000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic encapsulation adhesive films, and in particular to a metal corrosion inhibition encapsulation adhesive film, a preparation method, an application method and a photovoltaic module encapsulation component. Background Art
[0002] With the development of technology, the main grid technology of solar cells has developed from MBB and SMBB to 0BB (no main grid). The no main grid technology is a further upgrade of the SMBB technology, and its cost reduction advantage is obvious. The no main grid technology directly eliminates the main grid of the cell, and prepares the cell fine grid through silver-coated copper slurry, or uses the copper electroplating process to prepare the grid line, further reducing the silver consumption; in addition, the embedded circular copper welding belt is used to replace the silver main grid of the cell to derive the current in the component link. The diameter of the common welding belt of the MBB component is 0.2-0.4mm, while the diameter of the 0BB welding belt is only 0.2mm, the shading area is smaller, and the power of the component can be increased. At present, the no main grid technology is widely used in IBC, HJT, TOPCON and other batteries.
[0003] Problems with materials in busbar-free technology: The thin grid of busbar-free technology uses low-cost silver-coated copper paste or electroplated pure copper to replace the traditional pure silver thin grid. The battery pure silver main grid is also replaced by an embedded circular copper welding strip. The chemical properties of copper materials are more active than silver, and they are easily oxidized and corroded, and the conductivity is reduced, which puts higher requirements on packaging materials. Patent CN117701189A uses magnesium oxide as an acid-absorbing material to absorb acetic acid and water vapor from EVA, improving the problems of battery cell welding strip corrosion, battery cell blackening, and film delamination. However, the acetic acid generated during the aging process of EVA materials and raw materials will inevitably corrode the battery materials.
[0004] Problems with the busbar-free technology process: In the busbar-free mass production process, first apply glue dots (UV glue, hot melt glue and other adhesives) to solidify the entire solder strip on the battery cell using UV lamps, ovens and other equipment, and then achieve alloying of the solder strip and the battery cell through lamination. This solution is different from the welding glue dot solution in that it does not require welding, and can be fixed by glue dot or silk screen printing, and has strong stability. However, the conventional EVA and POE adhesive films currently used in the industry have low melting temperatures and high fluidity. When encapsulating components, the adhesive film material melts before the solder strip, and there is a problem of shadows under the solder strip during EL testing (the solder strip is wrapped by EVA and POE materials, and the solder strip cannot form a conductive connection with the battery cell). In order to solve this problem, the industry uses electron radiation to pre-crosslink the EVA and POE adhesive films to reduce the fluidity of the adhesive film to solve the shadow under the solder strip during EL testing. However, the pre-crosslinked adhesive film leads to insufficient bonding between the solder strip and the battery cell, poor component reliability, and complex processes and high costs. In addition, the busbar-less photovoltaic industry uses low-fluidity thermoplastic PVB film to solve the LE shadow problem, but the price of pure PVB film is high, which is not conducive to component cost reduction, efficiency improvement and application promotion.
[0005] In summary, the development of a metal corrosion inhibition packaging film and its preparation method for practical application is of great significance. Summary of the invention
[0006] In summary, the present invention is necessary to provide a metal corrosion-inhibiting encapsulation film that effectively prevents active metal materials from being oxidized and corroded, and the resulting photovoltaic cell has low PID power attenuation, thereby improving the long-term reliability of photovoltaic modules.
[0007] Necessarily, the present invention also provides a method for preparing the above-mentioned metal corrosion inhibition packaging film.
[0008] If necessary, the present invention also provides an application method of the above-mentioned metal corrosion inhibition packaging film.
[0009] More importantly, the present invention also provides a photovoltaic module packaging component.
[0010] The technical solution of the present invention is:
[0011] A metal corrosion-inhibiting packaging film comprises a thermosetting adhesive layer and a thermoplastic corrosion-inhibiting layer.
[0012] The heat-curing adhesive layer is composed of the following raw material components by weight: 100 parts of a cross-linkable base resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of an auxiliary cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer;
[0013] The thermoplastic corrosion inhibition layer is composed of the following raw material components by weight: 100 parts of thermoplastic base resin, 1-20 parts of plasticizer, 0.1-1 part of coupling agent, and 0.5-10 parts of corrosion inhibitor.
[0014] Wherein, the corrosion inhibitor is selected from one or both of formula A or B,
[0015]
[0016] In formulas [A] and [B]], R1, R2, and R3 are H, alkyl, aryl, or heterocyclic groups.
[0017] The corrosion inhibitor is composed of the following two substances A2 and B1, and the structural formula of A is
[0018] The structural formula of B is
[0019] The weight ratio of A to B is 1:1
[0020] Wherein, the cross-linkable matrix resin is selected from one or more of EVA, PVB, and POE resins.
[0021] Wherein, the thermoplastic matrix resin is selected from one or more of PVB resin, TPU resin, PVA resin, PA resin, PI resin and epoxy resin.
[0022] Wherein, the peroxide crosslinking agent is selected from one or more of tert-butyl peroxycarbonate-2-ethylhexyl ester, tert-amyl peroxy (2-ethylhexyl) carbonate, tert-butyl peroxybenzoate, tert-butyl peroxyacetate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, and diisopropylbenzene peroxide;
[0023] The auxiliary cross-linking agent is selected from one or more of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxyacrylate, and triallyl isocyanate;
[0024] The coupling agent is selected from one or more of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, vinyl tri-tert-butoxysilane, 3-glycidyloxypropyl trimethoxysilane, and γ-aminopropyl triethoxysilane;
[0025] The light stabilizer is selected from hindered amine light stabilizers, including one or more of bis-2,2,6,6-tetramethylpiperidinol sebacate, polysuccinic acid (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol) ester, and bis (2,2,6,6-tetramethyl-4-piperidinol) sebacate;
[0026] The plasticizer is selected from one or more of DOP, DOTP, hydrogenated DOTP, 3GO, DOA, DOS, and DBS.
[0027] Wherein, the thickness of the heat-curing adhesive layer is 0.30-0.60 mm, and the thickness of the thermoplastic corrosion-inhibiting layer is 10-200 μm.
[0028] A method for preparing the metal corrosion inhibition packaging film as described above, characterized in that it comprises the following steps:
[0029] Step 1, preparation of a heat-curing adhesive layer: by weight, 100 parts of a cross-linkable matrix resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of a co-cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer are placed in a horizontal mixer and stirred evenly, and then the stirred materials are put into a single-screw extruder controlled at a temperature of 70°C-110°C, and extruded and cast at the die head through a T-type distributor to prepare a heat-curing adhesive layer base film;
[0030] Step 2, preparation of corrosion inhibition layer glue: by weight, 100 parts of thermoplastic matrix resin, 1-20 parts of plasticizer, 0.1-1 parts of coupling agent, 0.5-10 parts of corrosion inhibitor are placed in a stirring tank, and then 100-1000 parts of solvent are added to the stirring tank and stirred to dissolve to obtain corrosion inhibition layer glue.
[0031] Step 3, preparation of metal corrosion-inhibiting packaging film: apply the corrosion-inhibiting layer glue of step 2 on any surface of the bonding layer base film of step 1 through a slit coating process, remove the solvent through oven drying, and form a thermoplastic corrosion-inhibiting layer on the base film, finally obtaining a metal corrosion-inhibiting packaging film with a double-layer structure.
[0032] Wherein, the solvent of the corrosion inhibition layer glue is selected from one or more of water, ethanol, isopropanol, xylene, acetone, dichloromethane, ethyl acetate, and DMF.
[0033] The application method of the metal corrosion-inhibiting packaging film as described above is applied to a photovoltaic module packaging without a main grid cell, the heat-curing adhesive layer of the metal corrosion-inhibiting packaging film contacts the photovoltaic glass or back panel, and the thermoplastic corrosion-inhibiting layer of the metal corrosion-inhibiting packaging film contacts the battery cell.
[0034] A photovoltaic assembly packaging assembly without a main grid cell, the structure of which comprises a photovoltaic front plate glass, a metal corrosion-inhibiting packaging film, a main grid-free cell string, a metal corrosion-inhibiting packaging film, and a photovoltaic back plate in sequence.
[0035] The photovoltaic front panel glass, metal corrosion-inhibiting packaging film, main-grid-free battery string, metal corrosion-inhibiting packaging film and photovoltaic back panel are combined by hot pressing.
[0036] Compared with the prior art, the metal corrosion-inhibiting packaging film provided by the present invention comprises a thermosetting adhesive layer and a thermoplastic corrosion-inhibiting layer, wherein the thermosetting adhesive layer is composed of the following raw material components by weight: 100 parts of a cross-linkable matrix resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of a co-cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer; the thermoplastic corrosion-inhibiting layer is composed of the following raw material components by weight: 100 parts of a thermoplastic matrix resin, 1-20 parts of a plasticizer, 0.1-1 parts of a coupling agent, and 0.5-10 parts of a corrosion inhibitor. The metal corrosion-inhibiting packaging film of the present invention effectively solves the problem of shadows under the soldering strip by forming a thermoplastic corrosion-inhibiting layer on the thermosetting adhesive layer, and the thickness of the thermoplastic layer only needs to be 10-200 microns, which is lower in cost than the traditional pure thermoplastic PVB packaging film>300 microns. When the component is packaged, the contact glass (or backplane) is a heat-cured adhesive layer of the film, which provides long-lasting and effective heat-cured bonding force; and the layer that adheres to the battery cell is a thermoplastic corrosion inhibition layer of the film. The high molecular weight thermoplastic material has the characteristics of low fluidity, which prevents the film material from filling between the welding ribbon and the battery cell during the lamination process (causing the welding ribbon and the battery cell to be short-circuited and non-conductive), which can effectively solve the problem of shadows under the welding ribbon during EL testing of main grid-free component packaging. The corrosion inhibitor contained in it can form a protective layer with the metal grid line, welding ribbon, conductive coating, and bus bar material on the surface of the battery, effectively preventing active metal materials from being oxidized and corroded, thereby improving the long-term reliability of photovoltaic components and having a low PID power attenuation rate. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with some specific embodiments. The specific embodiments are for further illustrating the present invention in detail, but are not intended to limit the protection scope of the present invention.
[0038] According to the above method, the following substances are prepared for corrosion inhibitor:
[0039] Prepared by the method of patent CN201510774530.6, the corrosion inhibitor structure is as follows [A-1]:
[0040]
[0041] The corrosion inhibitor was prepared by the method of patent CN103562323B and the structure of the obtained corrosion inhibitor is as follows [B-1]:
[0042]
[0043] Preparation method of [A-2]:
[0044] A mixture of 4,7-dibromo-1H-2-isobutylbenzotriazole (1.32 g, 4.0 mmol), 4-tert-butylphenylboronic acid (10.0 mmol), tetrakis(triphenylphosphine)palladium(0) (1.00 g, 0.86 mmol), sodium carbonate (2.12 g, 20 mmol) in water (15 mL), butanol (50 mL) and toluene (30 mL) was stirred vigorously and heated at 100° C. under argon for 16 hours. The reaction mixture was poured into water (300 mL), stirred for 30 minutes, and extracted with toluene / ethyl acetate / hexane (5:3:2, 500 mL). Volatiles were removed under reduced pressure and the residue was chromatographed (silica gel, hexane / dichloromethane, 1:1). The separated product was recrystallized from ethanol to obtain [A-2] as 4,7-bis(4-tert-butylphenyl)-2-isobutyl-1H-benzotriazole.
[0045]
[0046] [A-3] Preparation method, 4,7-dibromo-1H-2-isobutylbenzotriazole (1.32g, 4.0mmol), phenylboronic acid (10.0mmol), tetrakis(triphenylphosphine)palladium(0) (1.00g, 0.86mmol), sodium carbonate (2.12g, 20mmol) in water (15mL) solution, butanol (50mL) and toluene (30mL) were vigorously stirred and heated at 100°C under argon for 16 hours. The reaction mixture was poured into water (300mL), stirred for 30 minutes, and extracted with toluene / ethyl acetate / hexane (5:3:2, 500mL). Volatiles were removed under reduced pressure, and the residue was chromatographed (silica gel, hexane / dichloromethane, 1:1). The separated product was recrystallized from ethanol to obtain [A-3] as 4,7-bis(phenyl)-2-isobutyl-1H-benzotriazole:
[0047]
[0048] Preparation of metal corrosion inhibition packaging film in embodiments and comparative examples
[0049] Step 1, preparation of a heat-curing adhesive layer: according to the weight parts shown in Table 1, 100 parts of a cross-linkable matrix resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of a co-cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer are placed in a horizontal mixer and stirred evenly, and then the stirred materials are put into a single-screw extruder controlled at a temperature of 70°C-110°C, and a heat-curing adhesive layer base film of 0.3-0.6 mm is prepared by extrusion casting through a T-type distributor at the die head;
[0050] Step 2, preparation of corrosion inhibition layer glue: according to the weight parts shown in Table 1, 100 parts of thermoplastic matrix resin, 1-20 parts of plasticizer, 0.1-1 parts of coupling agent, 0.5-10 parts of corrosion inhibitor are placed in a stirring tank, and then 100-1000 parts of solvent are added to the stirring tank and stirred to dissolve to obtain corrosion inhibition layer glue.
[0051] Step 3. Preparation of metal corrosion-inhibiting packaging film: The corrosion-inhibiting layer glue of step 2 is coated on any surface of the bonding layer base film of step 1 through a slit coating process, and the solvent is removed by oven drying. The thickness of the coated glue is controlled by a slit coating device to form a 10-200μm thermoplastic corrosion-inhibiting layer on the base film, and finally a metal corrosion-inhibiting packaging film with a double-layer structure is obtained.
[0052] A lamination preparation method for a photovoltaic module packaging component without a main grid cell: the component lamination order: photovoltaic front panel glass, metal corrosion-inhibiting packaging film, main grid-free battery string (UV dispensing fixation), metal corrosion-inhibiting packaging film of the embodiment and comparative example, photovoltaic back panel, wherein the surface of the metal corrosion-inhibiting packaging film contacting the photovoltaic glass (or back panel) is an adhesive layer, and the surface of the metal corrosion-inhibiting packaging film contacting the battery cell is a thermoplastic corrosion-inhibiting layer.
[0053] Component lamination process: After the metal corrosion-inhibiting packaging films and batteries in the embodiments and comparative examples are laid, they are heated and laminated to form the samples to be tested, wherein the lamination process parameters are temperature 145° C., vacuuming for 6 minutes, pressurizing for 1 minute, and maintaining pressure for 12 minutes.
[0054] PID and EL appearance tests of the prepared battery: refer to the IEC61215 and IECIEC62804 standards, and the test results are described in Table 1.
[0055] Table 1
[0056]
[0057]
[0058] As can be seen from Table 1, Comparative Example 4 shows that pure EVA encapsulation film is not friendly to busbar-free battery modules. Due to the low melting point and high fluidity of EVA materials, when used for battery packaging without busbar UV dispensing, the EVA film material melts before the soldering tape during module lamination. After lamination, the EVA resin is filled between the soldering tape and the battery cell. The soldering tape cannot form a conductive connection with the battery cell. The IEC61215 standard is used to test the EL of the module, and the problem of shadows under the soldering tape is found. And after the IEC62804 standard PID288 test, it was found that the busbar, soldering tape, and fine grid were severely corroded, and the module power dropped by 25.1%.
[0059] As can be seen from Table 1, it can be seen from Comparative Examples 1-3 that a layer of thermoplastic TPU and PVB is coated on the base film of the EVA adhesive layer. After the components are laminated, the EL of the components is tested using the IEC61215 standard, and it is found that the problem of shadows under the welding strips has been solved. This shows that treating a layer of thermoplastic PVB and TPU materials on the EVA base film can effectively solve the EL shadow problem. However, no metal corrosion inhibitor components are added to the thermoplastic layers of Comparative Examples 1-3. After the components are tested using the IEC62804 standard PID288, it is found that the welding strips and fine grids are severely corroded, and the power of the components has dropped by between 10-18%. The problem of corrosion of the fine grids and welding strips on the surface of the main grid-free battery cannot be solved. However, compared with Comparative Example 4, the busbars are not corroded, which is an improvement over the pure EVA film.
[0060] As can be seen from Table 1, in Examples 1-7 and Comparative Examples 1-3, a layer of thermoplastic material is coated on the base film of the thermosetting adhesive layer. After the components are laminated, the EL of the components is tested using the IEC61215 standard, and it is found that the problem of shadows under the soldering strips is solved.
[0061] As shown in Table 1, in Example 3 and Example 5, 0.5 parts of metal corrosion inhibitor components were added to the thermoplastic layer, and the module was tested using the IEC62804 standard PID288, and it was found that the fine grid was slightly corroded, and the module power decreased by 5.4% and 7.2% respectively. Compared with Examples 1-3, the problem of corrosion of the fine grid and the metal material of the welding strip on the surface of the main grid-free battery was effectively solved.
[0062] As can be seen from Table 1, the thermoplastic glue coating materials of Examples 1, 2, 4, 6, and 7 contain 1.5 to 10 parts of corrosion inhibitors. After the components are tested using the IEC62804 standard PID288, no corrosion is found on the surface of the battery and the fine grid, and the power of the components drops by 2%-3%. Compared with Example 2, Example 4 uses a compound of two corrosion inhibitors, and the metal corrosion inhibition effect is better, which is reflected in that after the components are tested using the IEC62804 standard PID288, the power of Example 4 drops by less than 1%, and the test value only drops by 0.5%.
[0063] The corrosion inhibitor in the embodiment is composed of formula [A-2] / formula [B-1]=1:1, and its comprehensive effect is the best.
[0064] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A metal corrosion inhibition packaging film, characterized in that: Contains a thermosetting bonding layer and a thermoplastic corrosion inhibition layer. The heat-curing adhesive layer is composed of the following raw material components by weight: 100 parts of a cross-linkable base resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of an auxiliary cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer; The thermoplastic corrosion inhibition layer is composed of the following raw material components by weight: 100 parts of thermoplastic base resin, 1-20 parts of plasticizer, 0.1-1 part of coupling agent, and 0.5-10 parts of corrosion inhibitor.
2. The metal corrosion inhibition packaging film according to claim 1, characterized in that: The corrosion inhibitor is selected from one or both of formula A and formula B, In formulas [A] and [B]], R1, R2, and R3 are H, alkyl, aryl, or heterocyclic groups.
3. The metal corrosion inhibition packaging film according to claim 2, characterized in that: The corrosion inhibitor is composed of the following two substances A2 and B1, wherein the structural formula of A is The structural formula of B is The weight ratio of A to B is 1:
1.
4. The metal corrosion inhibition packaging film according to claim 2, characterized in that: The cross-linkable matrix resin is selected from one or more of EVA, PVB, and POE resins.
5. The metal corrosion inhibition packaging film according to claim 2, characterized in that: The thermoplastic matrix resin is selected from one or more of PVB resin, TPU resin, PVA resin, PA resin, PI resin and epoxy resin.
6. The metal corrosion inhibition packaging film according to claim 2, characterized in that: The peroxide crosslinking agent is selected from one or more of tert-butyl peroxycarbonate-2-ethylhexyl ester, tert-amyl peroxy (2-ethylhexyl) carbonate, tert-butyl peroxybenzoate, tert-butyl peroxyacetate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, and dicumyl peroxide; The auxiliary cross-linking agent is selected from one or more of triallyl isocyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, trimethylolpropane triethoxyacrylate, and triallyl isocyanate; The coupling agent is selected from one or more of vinyl trimethoxysilane, vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane, γ-methacryloxypropyl trimethoxysilane, vinyl tri-tert-butoxysilane, 3-glycidyloxypropyl trimethoxysilane, and γ-aminopropyl triethoxysilane; The light stabilizer is selected from hindered amine light stabilizers, including one or more of bis-2,2,6,6-tetramethylpiperidinol sebacate, polysuccinic acid (4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol) ester, and bis (2,2,6,6-tetramethyl-4-piperidinol) sebacate; The plasticizer is selected from one or more of DOP, DOTP, hydrogenated DOTP, 3GO, DOA, DOS, and DBS.
7. The metal corrosion inhibition packaging film according to claim 1, characterized in that: The thickness of the heat-curing adhesive layer is 0.30-0.60 mm, and the thickness of the thermoplastic corrosion-inhibiting layer is 10-200 μm.
8. A method for preparing a metal corrosion inhibition packaging film according to any one of claims 1 to 7, characterized in that The following steps are included: Step 1, preparation of a heat-curing adhesive layer: by weight, 100 parts of a cross-linkable matrix resin, 0.1-1 parts of a peroxide cross-linking agent, 0.1-1 parts of a co-cross-linking agent, 0.1-1 parts of a coupling agent, and 0.1-1 parts of a light stabilizer are placed in a horizontal mixer and stirred evenly, and then the stirred materials are put into a single-screw extruder controlled at a temperature of 70°C-110°C, and extruded and cast at the die head through a T-type distributor to prepare a heat-curing adhesive layer base film; Step 2, preparation of corrosion inhibition layer glue: by weight, 100 parts of thermoplastic matrix resin, 1-20 parts of plasticizer, 0.1-1 parts of coupling agent, 0.5-10 parts of corrosion inhibitor are placed in a stirring tank, and then 100-1000 parts of solvent are added to the stirring tank and stirred to dissolve to obtain corrosion inhibition layer glue. Step 3, preparation of metal corrosion-inhibiting packaging film: apply the corrosion-inhibiting layer glue of step 2 on any surface of the bonding layer base film of step 1 through a slit coating process, remove the solvent through oven drying, and form a thermoplastic corrosion-inhibiting layer on the base film, finally obtaining a metal corrosion-inhibiting packaging film with a double-layer structure.
9. The method for preparing the metal corrosion inhibition packaging film according to claim 8, characterized in that: The solvent of the corrosion inhibition layer glue is selected from one or more of water, ethanol, isopropanol, xylene, acetone, dichloromethane, ethyl acetate and DMF.
10. The method for applying the metal corrosion inhibition packaging film according to claims 1 to 9, characterized in that: The metal corrosion-inhibiting packaging film is applied to a photovoltaic module packaging without a main grid cell, wherein the heat-curing adhesive layer of the metal corrosion-inhibiting packaging film contacts the photovoltaic glass or back plate, and the thermoplastic corrosion-inhibiting layer of the metal corrosion-inhibiting packaging film contacts the cell sheet.
11. A photovoltaic module packaging assembly without a main grid cell, characterized in that: The structure comprises, in sequence, a photovoltaic front plate glass, a metal corrosion-inhibiting packaging film as described in any one of claims 1 to 7, a main grid-free battery string, a metal corrosion-inhibiting packaging film as described in any one of claims 1 to 7, and a photovoltaic back plate.
Citation Information
Patent Citations
Polymeric coated busbar tape for photovoltaic systems
CN103930499A
Anticorrosive photovoltaic packaging material EVA adhesive film and preparation method thereof
CN110093112A
Double-layer packaging adhesive film for N-type TOPCon and preparation method of double-layer packaging adhesive film
CN116769424A
Benzotriazole compounds, resin compositions using the same, and wavelength conversion layers