Sulfur-modified metal oxide (oxyhydrogen) self-supporting nano catalytic material prepared by utilizing electrochemical corrosion strategy and application of sulfur-modified metal oxide (oxyhydrogen) self-supporting nano catalytic material in electrolytic hydrogen production

Sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials are formed on commercial metal substrates through electrochemical corrosion methods, which solves the problems of low energy efficiency of OER catalysts and performance degradation caused by adhesive contact, and achieves high efficiency, Low-cost and environmentally friendly catalyst preparation suitable for electrolytic water hydrogen production technology.

CN118756218APending Publication Date: 2024-10-11CHENGDU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410916646.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing electrolysis water hydrogen production technology, the kinetics of the oxidation-reduction reaction (OER) is slow, resulting in low energy efficiency, the cost of noble metal catalysts is high, and the contact with binders of non-precious metal catalysts leads to a decrease in catalytic performance.

Method used

The electrochemical corrosion method is used to form sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials through the corrosion of chloride ions and the attraction of anions by using sodium chloride electrolyte and external electric field without using adhesives. , firmly anchored on a commercial metal substrate to form a highly active, long-life OER catalyst.

Benefits of technology

It achieves efficient, low-cost, and environmentally friendly OER catalyst preparation, avoids high temperature, high pressure, and multi-step synthesis, significantly improves catalytic activity and stability, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004935294220000011
    Figure HDA0004935294220000011
  • Figure HDA0004935294220000012
    Figure HDA0004935294220000012
  • Figure HDA0004935294220000013
    Figure HDA0004935294220000013
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic hydrogen production, and provides a sulfur-modified metal oxide (oxyhydrogen) self-supporting nano catalytic material and electro-catalysis application of the material by utilizing a simple, convenient and industrially compatible electrochemical corrosion strategy. According to the self-supporting catalytic material, a sodium chloride solution containing a sulfur source is used as an electrolyte, chloride ion corrosion is used as a tool, commercial foam ferronickel is used as an anode under the configuration of standard three electrodes, the commercial foam ferronickel is treated through a CV technology (the voltage window is 0-1 V vs.Hg / HgO), and then post-treatment is performed to obtain the self-supporting catalytic material. And after electrochemical corrosion, the vulcanized nanospheres are uniformly assembled on the surface of the commercial metal substrate. According to the innovative technology, the cheap commercial metal foam substrate can be quickly and simply converted into the high-activity and high-stability oxygen evolution catalyst. As chloride ions directly etch the metal support, the sulfur-functionalized metal oxide (oxyhydrogen) nanospheres are tightly combined with the commercial metal foam substrate. The nanospheres are uniformly and tightly arrayed on commercial substrate foam, and the problems of less reaction active phase exposure, low coordination structure, poor catalytic performance, performance degradation caused by active substance falling and the like in the existing OER electrocatalyst can be effectively solved. As the anode has a strong adsorption effect on anions, the electrochemical corrosion method can be expanded to a sodium chloride solution system containing a plurality of loading sources such as a sulfur source, a boron source and a phosphorus source so as to prepare the sulfur-modified metal oxide (oxyhydrogen) self-supporting nano catalytic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytic hydrogen production, and in particular to the rapid preparation of a sulfur-modified metal oxide (hydroxide) self-supporting electrocatalyst by an electrochemical corrosion method, and the application of the catalyst in hydrogen production by electrolytic water. Background Art

[0002] Hydrogen (H 2 As a green energy carrier, hydrogen has the characteristics of zero emission (the main product of hydrogen combustion is water, and the use of hydrogen does not produce harmful gases such as carbon dioxide), high energy density (the energy density of hydrogen is higher than that of fuel oil, which can provide more energy), renewable (can be produced by water electrolysis, biomass, solar energy, wind energy, etc.), and convenient storage (can appear in the form of liquid, solid, gas, metal hydride, etc., which can greatly meet various scenarios). Therefore, hydrogen energy is expected to replace traditional fossil fuels and alleviate problems such as energy crisis and environmental pollution.

[0003] The electrochemical oxygen evolution reaction (OER) is an electron-proton coupled four-electron transfer reaction with a theoretical thermodynamic potential (E) of 1.23 V. Its kinetics are slow, so a large amount of additional energy (called applied overpotential (η OER =EE O2 / OH>0.3V), resulting in a significant decrease in the energy efficiency of hydrogen production from water electrolysis. Therefore, overcoming the energy barrier of OER is crucial to realize closed-loop clean energy devices. The first but challenging task to achieve this goal lies in the development of excellent OER catalysts through more environmentally friendly and industrially compatible methods.

[0004] The study found that precious metal catalysts (IrO 2 , RuO 2 etc.) accelerate the OER reaction to a great extent, but their applications are limited due to their high cost and scarcity. In recent years, inexpensive, natural high-background non-precious metal catalysts (such as Ni, Fe) have attracted much attention and are regarded as a promising alternative to precious metal catalysts. Among various non-precious metal electrocatalysts, sulfur-modified metal oxides (hydroxides) have good conductivity and excellent oxygen evolution performance. The introduction of sulfur elements with high electronegativity can significantly enhance the degree of electron delocalization in the metal phase, provide an effective channel for metal cations to lose electrons, and reduce the energy barrier for conversion reactions in nanocatalytic materials.

[0005] However, most finely designed sulfur-metal catalysts are in powder form and need to be bonded to a current collector by a binder such as Nafion. This will severely block the electroactive sites, increase the electrode impedance, and hinder the electron / mass transfer. Worse, during long-term use, the insufficient adhesion of the current collector to the material leads to the fall-off of the reactive phase and a sharp drop in performance.

[0006] The development of binder-free and self-supporting OER catalysts can effectively solve these problems. The high conductivity of sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials ensures the rapid transfer of electrons, and the addition of no binder is conducive to the reactants entering the reaction center, improving the catalytic reaction activity. In recent years, hydrothermal, high-temperature annealing, plasma / laser technology has been used to prepare sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials. However, these methods usually require cumbersome procedures, excessive heat or electrical energy input, excessive budget, low yield, and sophisticated instruments, which ultimately leads to increasing difficulty in structure / performance adjustment and soaring production costs.

[0007] In order to circumvent the above shortcomings, the present invention uses an electrochemical corrosion method to firmly fix the sulfur-modified metal phase on a commercial metal substrate without using an adhesive to form a self-supporting OER catalyst. Harmful corrosion events in the seawater industry are turned into treasures. The high hygroscopicity, corrosiveness and permeability of chloride ions destroy the passivation film on the surface of commercial metal foams and release metal cations, which are further hydrolyzed into metal hydroxides. At the same time, under the action of an external electric field, anionic groups (such as sulfur-containing anions) move to the anode surface (commercial metal foam), and while generating metal oxides (hydroxides), they are functionalized to form sulfur-modified metal oxides (hydroxides) with high catalytic activity. Self-supporting nanocatalytic materials. Such industrially scalable methods for rapid preparation of sulfur-metal catalysts are rarely reported. Summary of the invention

[0008] Technical problems solved by the present invention:

[0009] The harmful corrosion events that were originally in the natural environment are transformed into a catalytic material preparation method (electrochemical corrosion method), and the problems of sulfur functionalization of OER catalysts, cumbersome processes, high costs, environmental unfriendliness, and weak catalyst-substrate contact leading to decreased catalytic performance are solved.

[0010] The technical solution adopted by the present invention is:

[0011] With the idea of ​​turning waste into treasure, a simple method that can be industrialized is provided by using the chloride ion corrosion of the load source - sodium chloride electrolyte in the electrochemical process and the electrostatic attraction of the anode to the anion as tools (electrochemical corrosion method) to quickly prepare a sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material and its application in the field of electrolytic hydrogen production.

[0012] The specific contents are as follows:

[0013] First, the present invention provides a sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material, in which the sulfur-modified nanometal particles are uniformly anchored on the surface of a commercial metal substrate.

[0014] The catalytic material is obtained by treating a commercial metal substrate by a CV method (voltage window of 0-1V (Vvs.Hg / HgO)) using a load source - sodium chloride as an electrolyte, a standard three-electrode configuration, commercial metal foam as an anode, mercury / mercury oxide (Hg / HgO) as a reference electrode, and a platinum plate as a counter electrode.

[0015] The loading source includes a sulfur source and / or a boron source and a phosphorus source. The metal substrate obtained by the CV treatment is rinsed with deionized water and dried. The treatment time of the metal substrate in the CV treatment is about 1 minute.

[0016] In the present invention, the diameter of the nanoparticles composed of nanosheets is about 0.67 μm; the gap between adjacent nanosheets is about 0.05 to 0.27 μm; and the gap between adjacent nanoparticles is about 0.06 to 1.22 μm.

[0017] In the present invention, the surface of the nanosphere is rich in mesoporous structure.

[0018] In the present invention, the load source can be dissolved in a sodium chloride solution; the electrolyte includes the following features: the load source can be any one of a sulfur source, a boron source, and a phosphorus source. When the load source is a sulfur source, the sulfur source includes any one of potassium thiocyanate, ammonium persulfate, sodium thiosulfate, sodium sulfide, and thiourea; when it is a boron source, the boron source includes boric acid. When it is a phosphorus source, the phosphorus source includes sodium dihydrogen phosphate.

[0019] In the above-mentioned electrolyte, when the load source is a sulfur source, the molar concentration ratio of the sulfur source to sodium chloride is 0-0.2mol / L:3mol / L; when the load source is a boron source, the molar concentration ratio of the boron source to sodium chloride is 0.2mol / L:3mol / L; when the load source is a phosphorus source, the molar concentration ratio of the phosphorus source to sodium chloride is 0.2mol / L:3mol / L.

[0020] Second, the present invention provides the use of the aforementioned sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material in hydrogen production by water electrolysis.

[0021] The present invention exploits harmful corrosion events to rapidly convert inexpensive commercial metal foams into highly active, long-life oxygen evolution catalysts.

[0022] Using a sulfur source-sodium chloride solution as the electrolyte, the high hygroscopicity, corrosiveness and permeability of chloride ions are used to break down the passivation film on the surface of commercial metal foams to form metal oxides (hydroxides). At the same time, under the action of an external electric field, anionic groups (such as sulfur-containing anions) move toward the anode (commercial metal substrate) and firmly combine with the metal oxides (hydroxides) to form sulfur-modified metal oxides (hydroxides) self-supporting nanocatalytic materials. The originally smooth surface of the commercial metal substrate is modified by sulfur-metal nanoparticles and becomes rough. This structure is conducive to the diffusion and penetration of the electrolyte and helps the bubbles to detach from the catalyst surface. In addition, the self-supporting catalyst avoids the use of binders, and the material surface can expose more active sites, have lower electrode resistance and higher mass / charge transfer efficiency.

[0023] The commercial metal substrate reacts directly with the solution by directly etching the metal support, and the sulfur-containing anions are quickly connected to the metal oxide (hydroxide) layer under the drive of electric potential. This strong catalyst-substrate contact ensures the long-term catalytic stability of the sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material.

[0024] The present invention uses a cheap, low-toxic sulfur source-sodium chloride solution as an electrolyte, and performs repeated CV treatment in a 0-1V (vs.Hg / HgO) voltage window, and can produce a sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material with high catalytic activity and long service life in high yield within 2 minutes at the fastest. The method effectively avoids harsh synthesis conditions such as high pressure and high temperature, strong acid and alkali, long preparation time, multiple steps, and strict environment. The synthesis method has the advantages of high repeatability, cheap synthetic raw materials, simple operation, easy amplification, short preparation cycle, and low energy consumption. Therefore, it has a broader prospect for industrial application.

[0025] The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material (labeled as NFF-S1) obtained by the present invention x A y @mn; where S1 represents potassium thiocyanate, x is the molar concentration of the sulfur source, A represents sodium chloride, y is the molar concentration of sodium chloride, m is the electrolyte temperature, and n is the number of CV cycles) has a distinct three-dimensional hierarchical structure, abundant electroactive sites, excellent conductivity, strong interfacial bonding, and significant electronic structure modification effect, providing excellent and stable OER performance. 0.2M potassium thiocyanate-3M sodium chloride solution was CV scanned for 3 cycles at 40°C (NFF-S1 0.2 A 3 @40℃-3) as an example, at 10mAcm -2 , 50mAcm -2 and 100mAcm -2At the current density of 2.5, the overpotentials are 230.18mV, 259.23mV and 276.53mV respectively, which are better than the metal oxide (hydroxide) obtained by pure sodium chloride corrosion (NFF-A 3 @40℃-3) catalyst (286.63mV, 349.00mV and 380.32mV). In the constant voltage polarization test, NFF-S1 0.2 A 3 @40℃-3 can be at 1Acm -2 It can work stably for at least 549.45 hours at industrial-grade current density without obvious performance degradation, which indicates that the OER activity of sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials prepared by electrochemical corrosion strategy is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is the LSV test result diagram of oxygen evolution reaction of each test sample;

[0027] Figure 2 for Figure 1 The enlarged image of the inner black dotted box;

[0028] Figure 3 The catalyst (NFF-S1 x A y @mn、NFF-A 3 @40℃-3) LSV polarization curve;

[0029] Figure 4 For NFF-S1 x A y @mn、NFF-A 3 @40℃-3 Overpotential of oxygen evolution reaction (OER);

[0030] Figure 5 For NFF-S1 0.2 A 3 @40℃-3 stability test chart.

[0031] Figure 6 The catalyst (NFF-S2 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve;

[0032] Figure 7 For NFF-S2 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3 OER reaction overpotential;

[0033] Figure 8 The catalyst (NFF-S3 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve;

[0034] Fig. 9 For NFF-S3 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3 OER reaction overpotential;

[0035] Fig.10 The catalyst in Example 4 (NFF-S4 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve.

[0036] Fig.11 For NFF-S4 0.2 A 3 @40℃-3、NFF-A 3 OER reaction overpotential @40℃-3.

[0037] Fig.12 The catalyst (NFF-S5 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve.

[0038] Fig.13 For NFF-S5 0.2 A 3 @40℃-3、NFF-A 3 OER reaction overpotential @40℃-3.

[0039] Fig.14 The catalyst (NFF-B 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve.

[0040] Fig.15 NFF-B 0.2 A 3 @40℃-3、NFF-A 3 OER reaction overpotential @40℃-3.

[0041] Fig.16 The catalyst (NFF-P 0.2A 3 @40℃-3、NFF-A 3 @40℃-3) LSV polarization curve.

[0042] Fig.17 NFF-P 0.2 A 3 @40℃-3、NFF-A 3 @40℃-3(OER) reaction overpotential;

[0043] Fig.18 For NFF-S1 0.2 A 3 @40℃-3 and NFF-A 3 @40℃-3 Before and after activation (NFF-S1 0.2 A 3 @40℃-3-ac and NFF-A 3 @40℃-3-ac) SEM image

[0044] Fig.19 NFF-A 3 @40℃-3Elemental Mapping before activation

[0045] Fig. 20 NFF-A 3 @40℃-3Elemental Mapping after activation

[0046] Fig.21 For NFF-S1 0.2 A 3 @40℃-3Elemental Mapping before activation

[0047] Fig. 22 For NFF-S1 0.2 A 3 @40℃-3Elemental Mapping after activation DETAILED DESCRIPTION

[0048] In order to more clearly explain the purpose, technical scheme and advantages of the embodiments of the present invention, the technical scheme in the embodiments will be described in detail below. If specific conditions are not particularly specified, the operation will be carried out according to the usual conditions or the recommendations of the manufacturer. When the manufacturer of the reagent or instrument is not particularly specified, it refers to the conventional products that can be purchased on the market.

[0049] Example 1

[0050] Sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material, and its preparation method, comprising the following steps: dissolving 0-0.01 mol potassium thiocyanate and 0.15 mol sodium chloride in 50 ml of deionized water to obtain an electrolyte. Heat the electrolyte to 30-50°C and keep it warm, and use a standard three-electrode configuration to use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as an anode, mercury / mercury oxide (Hg / HgO) as a reference electrode, and a platinum plate as a counter electrode. Within the voltage window range of 0-1V (vs.Hg / HgO), CV cycles are performed for several cycles. Remove the treated commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material (sample labeled NFF-S1 x A y @mn; S1 represents potassium thiocyanate, x represents the molar concentration of potassium thiocyanate, A represents sodium chloride, y represents the molar concentration of sodium chloride, m represents the electrolyte insulation temperature, and n represents the number of CV cycles). The sample under the optimal synthesis conditions is marked as NFF-S1 0.2 A 3 @40℃-3 (i.e. 0.2mol / L potassium thiocyanate, 3mol / L sodium chloride CV cycle 3 times in 40℃ electrolyte).

[0051] The proportions of the specific parameters in Example 1 are shown in Table 1.

[0052] Table 1 Parameter ratio table

[0053]

[0054] Example 2

[0055] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol ammonium persulfate and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a standard three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. Repeat CV for several cycles within the voltage window range of 0-1V (vs.Hg / HgO). Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-S2 0.2 A 3 @40℃-3;S2 0.2 Indicates 0.2 mol / L ammonium persulfate, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0056] The ratio of each specific parameter in Example 2 is shown in Table 2

[0057] Table 2 Parameter ratio table

[0058]

[0059]

[0060] Example 3

[0061] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol sodium thiosulfate and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. Within the voltage window range of 0-1V (vs.Hg / HgO), CV scan several times. Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-S3 0.2 A 3 @40℃-3;S3 0.2 Indicates 0.2 mol / L sodium thiosulfate, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0062] The ratio of each specific parameter in Example 3 is shown in Table 3

[0063] Table 3 Parameter ratio table

[0064]

[0065] Example 4

[0066] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol sodium sulfide and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. CV scans several times within the voltage window range of 0-1V (vs.Hg / HgO). Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-S4 0.2 A 3 @40℃-3;S40.2 Indicates 0.2 mol / L sodium sulfide, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0067] The ratio of each specific parameter in Example 4 is shown in Table 4

[0068] Table 4 Parameter ratio table

[0069]

[0070] Example 5

[0071] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol thiourea and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. CV scans are performed for several cycles within the voltage window range of 0-1V (vs.Hg / HgO). Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-S5 0.2 A 3 @40℃-3;S5 0.2 Indicates 0.2 mol / L thiourea, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0072] The ratio of each specific parameter in Example 5 is shown in Table 5

[0073] Table 5 Parameter ratio table

[0074]

[0075] Example 6

[0076] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol boric acid and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. Within the voltage window range of 0-1V (vs.Hg / HgO), CV scans are performed for several cycles. Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-B 0.2 A 3 @40℃-3;B 0.2 Indicates 0.2 mol / L boric acid, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0077] The ratio of each specific parameter in Example 6 is shown in Table 6

[0078] Table 6 Parameter ratio table

[0079]

[0080]

[0081] Example 7

[0082] The difference between this embodiment and embodiment 1 is that its preparation method comprises the following steps: dissolving 0-0.01 mol sodium dihydrogen phosphate and 0.15 mol sodium chloride in 50 mL of deionized water to obtain an electrolyte. Heat the electrolyte to 40°C and keep it warm. Using a three-electrode configuration, use commercial nickel-iron foam (NFF) (Kunshan Dingsheng Chemical Materials Co., Ltd., Ni:Fe=7:3) as the anode, Hg / HgO as the reference electrode, and a platinum plate as the counter electrode. CV scans several times within the voltage window range of 0-1V (vs.Hg / HgO). Remove the corroded commercial nickel-iron foam, rinse with deionized water, wipe off the attached liquid with filter paper, and air-dry at room temperature to obtain a sample (the sample is labeled NFF-P 0.2 A 3 @40℃-3;P 0.2 Indicates 0.2 mol / L sodium dihydrogen phosphate, A 3 represents 3 mol / L sodium chloride, 40°C is the electrolyte insulation temperature, and 3 is the number of CV cycles).

[0083] The ratio of each specific parameter in Example 7 is shown in Table 7

[0084] Table 7 Parameter ratio table

[0085]

[0086] <Test example>

[0087] 1.CV, LSV and EIS tests

[0088] The performance of the sulfur (boron, phosphorus) modified metal oxide (hydroxide) self-supporting nanocatalytic materials in Examples 1-7 was tested.

[0089] The test process is as follows: in 1M KOH electrolyte (prepared with deionized water), a standard three-electrode configuration is used for performance testing, sulfur (boron, phosphorus) modified metal oxide (hydroxide) self-supporting nanocatalytic material is used as the anode, mercury / mercury oxide electrode is used as the reference electrode, and platinum plate is used as the cathode. Wuhan Coster Corrtest Studio 6 electrochemical workstation is used to test the oxygen evolution reaction (OER) performance of the electrocatalytic material at room temperature.

[0090] The test results are shown in Table 8 and Figure 1 (In order to more intuitively distinguish each LSV curve, we enlarged Figure 1 The black dashed box area is marked as Figure 2 ), the results showed that sulfur (boron, phosphorus) modified metal oxide (hydroxide) self-supporting nanocatalytic materials were successfully prepared by electrochemical corrosion, and their OER performance was significantly improved.

[0091] The CV cycle number and electrolyte holding temperature were studied to determine the optimal synthesis conditions. In the study of the optimal CV cycle number, the catalyst NFF-S1 was compared 0.2 A 3 @40℃-3(1-1), NFF-S1 0.2 A 3 @40℃-2(1-2) and NFF-S1 0.2 A 3 @40℃-4(1-3) OER performance, the results show a typical volcano type, and the sample obtained by 3 cycles of CV treatment has the best performance. In the study of the optimal electrolyte insulation temperature, NFF-S1 was compared 0.2 A 3 @40℃-3(1-1), NFF-S1 0.2 A 3 @30℃-3(1-4) and NFF-S1 0.2 A 3@50℃-3(1-5) OER performance, the results show a typical platform type, the OER activity of the catalytic material obtained by 3 cycles of CV treatment at 40℃ and 50℃ is almost the same, but significantly higher than the sample prepared at 30℃. From the perspective of energy saving and emission reduction, 40℃ is considered as the optimal electrolyte insulation temperature. That is, the optimal synthesis conditions are that the electrolyte is prepared with 0.2mol / L potassium thiocyanate and 3mol / L sodium chloride, kept at 40℃, and CV cycled 3 times in the voltage window range of 0-1V (vs.Hg / HgO) (marked as NFF-S1 0.2 A 3 @40℃-3).

[0092] Table 8 Oxygen evolution overpotential test results

[0093]

[0094]

[0095] The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material (NFF-S1 0.2 A 3 @40℃-3(1-1), NFF-S1 0.2 A 3 @40℃-2(1-2), NFF-S1 0.2 A 3 @40℃-4(1-3), NFF-S1 0.2 A 3 @30℃-3(1-4), NFF-S1 0.2 A 3 @50℃-3(1-5)) and metal oxide (hydroxide) NFF-A 3 @40℃-3(1-6) for performance testing.

[0096] The test process is the same as above, and CV, LSV, EIS and it tests are performed. The test results are shown in Figure 3-Figure 5 .

[0097] Figure 3 The LSV polarization curves of 1-1 to 1-6 are shown in Figure 1. It can be seen from the figure that the sulfur-modified metal oxide (hydroxide) compounds (1-1 to 1-5) exhibit excellent OER performance. At low current density, the starting potential of the sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials (1-1 to 1-5) is significantly lower than that of the metal oxide (hydroxide) NFF-A. 3 @40℃-3(1-6), with the increase of voltage, the increase of current density of sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials (1-1~1-5) is relatively 3 @40℃-3(1-6) is more obvious.

[0098] Figure 4 is the overpotential diagram, from Figure 4 (Based on NFF-S1 0.2 A 3 @40℃-3(1-1) and NFF-A 3 @40℃-3(1-6) as an example) NFF-S1 can be obtained 0.2 A 3 @40℃-3(1-1) at 10mA cm -2 , 50mA cm -2 and 100mA cm -2 At different current densities, the overpotentials are 230.18mV, 259.23mV and 276.53mV respectively, which are better than NFF-A. 3 @40℃-3(1-6)(286.63mV, 349.00mV and 380.32mV).

[0099] Figure 3 and Figure 4 It is further shown that the sulfidation of metal oxides (hydroxides) by electrochemical corrosion can significantly improve the catalytic activity of the catalyst.

[0100] Figure 5 This is the constant potential polarization curve of NFF-S10.2A3@40℃-3, with a current of 1A cm -2 Industrial current density, NFF-S1 0.2 A 3 @40℃-3 can run stably for at least 549.45 hours. Such an extremely long operating life reflects the excellent structural stability of the catalytic material and indicates the great potential of electrolyzing water to produce practical fuel gas at commercial current density.

[0101] The sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S2 in Example 2 0.2 A 3 @40℃-3(2-1), metal oxide (hydroxide) NFF-A 3 @40℃-3(2-2) OER performance test

[0102] The test process is the same as above, and CV, LSV, and EIS tests are performed. The test results are shown in Figure 6-Figure 7 .

[0103] Figure 6 For NFF-S2 0.2 A 3 @40℃-3(2-1) and NFF-A 3 @40℃-3(2-2) LSV polarization curve. It can be seen from the figure that NFF-S20.2 A 3 @40℃-3(2-1) has better OER performance than NFF-A 3 @40℃-3(2-2), Sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S2 at the same current density 0.2 A 3 @40℃-3(2-1) has a lower overpotential than the metal oxide (hydroxide) catalyst NFF-S2 0.2 A 3 @40℃-3(2-2).

[0104] Figure 7 is the overpotential diagram, from Figure 7 It can be seen that NFF-S2 0.2 A 3 @40℃-3(2-1) at 10mA cm -2 , 50mA cm -2 and 100mA cm -2 At the current density, the overpotentials are 278.60mV, 318.75mV and 342.50mV respectively, which are better than the metal oxide (hydroxide) catalyst NFF-A. 3 @40℃-3(2-2)(286.63mV, 349.00mV and 380.32mV).

[0105] Figure 6-Figure 7 It is further shown that the electrochemical corrosion method can dope different sulfides (ammonium persulfate) into metal oxides (hydroxides).

[0106] The sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S3 in Example 3 0.2 A 3 @40℃-3(3-1), metal oxide (hydroxide) NFF-A 3 @40℃-3(3-2) for OER performance test.

[0107] The test process is the same as above, and CV, LSV and EIS tests are performed. The test results are shown in Figure 8-Figure 9 .

[0108] Figure 8 For NFF-S3 0.2 A 3 @40℃-3(3-1) LSV polarization curve. It can be seen from the figure that NFF-S3 0.2 A 3 @40℃-3(3-1) also has excellent OER performance, which is comparable to metal oxide (hydroxide) NFF-A 3 @40℃-3(3-2)Compared with NFF-S3 at the same current density0.2 A 3 @40℃-3(3-1) has a smaller overpotential.

[0109] Fig. 9 is the overpotential diagram, from Fig. 9 You can get NFF-S3 0.2 A 3 @40℃-3(3-1) at 10mA cm -2 , 50mA cm -2 and 100mA cm -2 At the current density, the overpotentials are 238.41mV, 273.43mV and 297.70mV respectively, which are better than the metal oxide (hydroxide) NFF-A without sulfurization. 3 @40℃-3(3-2)(286.63mV, 349.00mV and 380.32mV). This means that metal oxides (hydroxides) can still be sulfided by electrochemical corrosion when sodium thiosulfate is used as the sulfur source.

[0110] Figure 8-Figure 9 It is further shown that what is more important is that currently, different sulfur sources (sodium thiosulfate) can be incorporated into metal oxides (hydroxides) using the electrochemical corrosion method to obtain OER catalytic materials with higher catalytic activity.

[0111] The sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S4 in Example 4 0.2 A 3 @40℃-3(4-1), Metal Oxide (Hydroxide) NFF-A 3 @40℃-3(4-2) for OER performance test.

[0112] The test process is the same as above, and CV, LSV, and EIS tests are performed. The test results are shown in Figure 10-11 .

[0113] Fig.10 For NFF-S4 0.2 A 3 @40℃-3(4-1) and NFF-A 3 @40℃-3(4-2) LSV polarization curve. It can be seen from the figure that NFF-S4 0.2 A 3 @40℃-3(4-1) has excellent OER performance. At the same current density, NFF-S4 0.2 A 3 @40℃-3(4-1) has a significantly lower overpotential than NFF-A 3 @40℃-3(4-2).

[0114] Fig.11is the overpotential diagram, from Fig.11 It can be seen that NFF-S4 0.2 A 3 @40℃-3(4-1) at 10mA cm -2 , 50mAcm -2 and 100mA cm -2 At the current density, the overpotentials are 238.21mV, 283.89mV and 311.22mV, which are significantly lower than those of NFF-A. 3 @40℃-3(4-2)(286.63mV, 349.00mV and 380.32mV).

[0115] Figure 10-11 It is further shown that what is more important is that currently, different sulfur sources (sodium sulfide) can be incorporated into metal oxides (hydroxides) using the electrochemical corrosion method to obtain OER catalytic materials with higher catalytic activity.

[0116] The sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S5 in Example 5 0.2 A 3 @40℃-3(5-1), metal oxide (hydroxide) NFF-A 3 @40℃-3(5-2) for OER performance test.

[0117] The test process is the same as above, and CV, LSV, and EIS tests are performed. The test results are shown in Figure 12-13 .

[0118] Fig.12 For NFF-S5 0.2 A 3 @40℃-3(5-1) and NFF-A 3 @40℃-3(5-2) LSV polarization curve. It can be seen from the figure that NFF-S5 0.2 A 3 @40℃-3(5-1) has better OER performance.

[0119] Fig.13 For NFF-S5 0.2 A 3 @40℃-3(5-1) and NFF-A 3 @40℃-3(5-2) overpotential diagram, from Fig.13 Available NFF-S5 0.2 A 3 @40℃-3(5-1) at 10mA cm -2 , 50mA cm -2 and 100mA cm -2At the current density of 2.547 W, the overpotentials are 252.18 mV, 287.37 mV and 311.62 mV respectively, which is better than that of metal oxide (hydroxide) NFF-A. 3 @40℃-3(5-2).

[0120] Figure 12-13 It is further shown that what is more important is that different sulfur sources (thiourea) can be incorporated into metal oxides (hydroxides) using the electrochemical corrosion method to obtain OER catalytic materials with higher catalytic activity.

[0121] The boron-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-BA in Example 6 3 @40℃-3(6-1), metal oxide (hydroxide) NFF-A 3 @40℃-3(6-2) for performance testing.

[0122] The test process is the same as above, and CV, LSV, and EIS tests are performed. The test results are shown in Figure 14-15 .

[0123] Fig.14 For NFF-BA 3 @40℃-3(6-1) and NFF-A 3 @40℃-3(6-2) LSV polarization curve. It can be seen from the figure that NFF-BA 3 @40℃-3(6-1) has better OER performance.

[0124] Fig.15 For NFF-BA 3 @40℃-3(6-1) and NFF-A 3 @40℃-3(6-2) overpotential diagram, Fig.15 NFF-BA available 3 @40℃-3(6-1) at 10mA cm -2 , 50mA cm -2 and 100mAcm -2 At current densities of 2.3 and 1.6, the overpotentials are 249.58 mV, 286.52 mV and 310.31 mV, respectively, which are better than those of metal oxide (hydroxide) NFF-A. 3 @40℃-3(6-2).

[0125] Figure 14-15 It is further shown that what is more important is that the electrochemical corrosion method can not only incorporate sulfur sources into metal oxides (hydroxides), but also incorporate boron sources into metal oxides (hydroxides) to obtain OER catalytic materials with higher catalytic activity.

[0126] The phosphorus-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-PA in Example 7 3 @40℃-3(7-1), metal oxide (hydroxide) NFF-A 3 @40℃-3(7-2) for performance test.

[0127] The test process is the same as above, and CV, LSV, and EIS tests are performed. The test results are shown in Figure 16-Figure 17 .

[0128] Fig.16 For NFF-PA 3 @40℃-3(7-1) and NFF-A 3 @40℃-3(7-2) LSV polarization curve. It can be seen from the figure that NFF-PA 3 @40℃-3(7-1) has better OER performance.

[0129] Fig.17 For NFF-PA 3 @40℃-3(7-1) and NFF-A 3 @40℃-3(7-2) overpotential diagram, Fig.17 Available NFF-PA 3 @40℃-3(7-1) at 10mAcm -2 , 50mAcm -2 and 100mA cm -2 At the current density, its overpotential is 268.90mV, 307.33mV and 329.39mV respectively, which is better than the metal oxide (hydroxide) NFF-A 3 @40℃-3(7-2).

[0130] Figure 16-Figure 17 It is further shown that what is more important is that the electrochemical corrosion method can not only incorporate sulfur sources (boron sources) into metal oxides (hydroxides), but also incorporate phosphorus sources into metal oxides (hydroxides) to obtain OER catalytic materials with higher catalytic activity.

[0131] comprehensive Figure 1-17 It is proved that the rapid electrochemical corrosion method is a synthetic method with wide adaptability. The present invention makes full use of the electrochemical corrosion method to successfully incorporate a sulfur source (potassium thiocyanate, ammonium persulfate, sodium thiosulfate, sodium sulfide, thiourea), a boron source (boric acid), and a phosphorus source (sodium dihydrogen phosphate) into the metal oxide (hydroxide) and form a stable, highly catalytically active sulfur (boron, phosphorus) modified metal oxide (hydroxide) active phase.

[0132] 2. Microstructure and chemical properties

[0133] The sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S1 in Example 1 0.2 A 3 @40℃-3(1-1), NFF-A 3 @40℃-3(1-6) and NFF were used as examples to analyze their microstructure and chemical properties. The specific results are shown in Figure 18-Figure 22 .

[0134] Fig.18 For NFF-S1 0.2 A 3 @40℃-3(1-1),NFF-A 3 @40℃-3(1-2) Before and after activation (NFF-S1 0.2 A 3 @40℃-3-ac, NFF-A 3 @40℃-3-ac) SEM image (the inset is the corresponding catalyst magnification image). Due to the chloride ion etching of commercial metal nickel iron foam ( Fig.18 d), passivation film on commercial metal foam surface ( Fig.18 e) is destroyed, accompanied by the generation of nanosheets ( Fig.18 a), after sulfidation, the nanosheets are modified by sulfide to form nanoparticles ( Fig.18 c). After activation, the catalyst surface undergoes a topological transformation ( Fig.18 b, d).

[0135] Fig.19 , 20 is metal oxide (hydroxide) NFF-A 3 @40℃-3(1-2) Elemental Mapping of Nanocatalytic Material before and after Activation. The figure shows that Ni, Fe, and O elements are evenly distributed on the surface of the material, reflecting that nickel iron oxide (hydroxide) is evenly distributed throughout the catalyst.

[0136] Fig.21 , 22 is a sulfur-modified metal oxide (hydroxide) self-supporting nanomaterial NFF-S1 0.2 A 3 @40℃-3(1-1) Elemental Mapping before and after activation. The figure shows that Ni, Fe, O, and S elements are evenly distributed on the surface of the material, reflecting that the electrochemical corrosion method can successfully sulfidize metal oxides (hydroxides), and the sulfur-modified metal phase is evenly distributed on the commercial metal foam.

[0137] The above analysis shows that the rapid electrochemical corrosion method provided by the present invention can not only quickly sulfurize the surface of commercial metal foam, but also boride and phosphate the commercial metal foam to form a unique nanoparticle array structure and exhibit excellent and stable electrochemical oxygen evolution performance.

[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material, characterized in that: Sulfur-modified metal oxide (hydroxide) nanospheres are evenly distributed on the surface of commercial metal substrate (nickel iron foam); Sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic materials are prepared using a standard three-electrode configuration, with a commercial metal foam substrate (nickel iron foam) as the anode, mercury / mercury oxide (Hg / HgO) as the reference electrode, and a platinum plate as the counter electrode. The sulfur source-sodium chloride electrolyte is kept at a certain temperature and then treated by CV technology (voltage window of 0-1V (vs.Hg / HgO)), and then post-treated.

2. The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to claim 1, characterized in that: The diameter of the sulfur-modified metal nanoparticles is about 0.67 μm.

3. The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to claim 1, characterized in that: The gap between adjacent nanosheets is 0.05-0.27 μm; the gap between adjacent nanoparticles is 0.06-1.22 μm.

4. The self-supporting metal sulfide nanocatalytic material according to claim 1, characterized in that: The surface of nanoparticles is rich in mesoporous structures.

5. The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to claim 1, characterized in that: The metal substrate includes nickel-iron foam.

6. The sulfur (boron, phosphorus) modified metal oxide (hydroxide) self-supporting nanocatalytic material according to any one of claims 1 to 5, characterized in that: The load sources can all be dissolved in sodium chloride solution; The load source-sodium chloride electrolyte includes at least one of the features (1-1) to (1-4): (1-1) The loading source includes any one of a sulfur source, a boron source, and a phosphorus source. (1-2) the loading source includes a sulfur source, and the sulfur source includes at least one of potassium thiocyanate, ammonium persulfate, sodium thiosulfate, sodium sulfide, and thiourea; (1-3) The loading source includes a boron source, and the boron source includes boric acid; (1-4) The loading source includes a phosphorus source, and the phosphorus source includes sodium dihydrogen phosphate.

7. The sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to any one of claim 6, characterized in that: In the electrolyte, the molar concentration ratio of the sulfur source to the sodium chloride is 0-0.2 mol / L:3 mol / L.

8. The boron-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to any one of claim 6, characterized in that: In the electrolyte, the molar concentration ratio of the boron source to sodium chloride is 0-0.2 mol / L:3 mol / L.

9. The phosphorus-modified metal oxide (hydroxide) self-supporting nanocatalytic material according to any one of claim 6, characterized in that: In the electrolyte, the molar concentration ratio of the phosphorus source to sodium chloride is 0-0.2 mol / L:3 mol / L.

10. Use of the sulfur-modified metal oxide (hydroxide) self-supporting nanocatalytic material as claimed in any one of claims 1 to 9 in hydrogen production by electrolysis.