Waterproof breathable synthetic leather and preparation method thereof
By using silver-loaded biomass activated carbon and breathable additives in polyurethane synthetic leather, combined with water-based polyurethane resin and cross-linking agents, a uniform breathable microporous structure is formed, which solves the gap in moisture absorption and breathability of traditional synthetic leather and achieves waterproofing The improved breathability and antibacterial effect extend the service life and reduce production costs.
Patent Information
- Application Number
- CN202410751687.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
Smart Images

Figure BDA0004888186360000131 
Figure BDA0004888186360000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic leather, and in particular relates to waterproof and breathable synthetic leather and a preparation method thereof. Background Art
[0002] Polyurethane synthetic leather has the advantages of high strength, wear resistance, cold resistance, breathability, aging resistance, solvent resistance, soft texture, beautiful appearance, and good processing performance. It is an ideal imitation leather product to replace natural leather. In recent years, polyurethane synthetic leather has been widely used in clothing, footwear, luggage, furniture and other industries.
[0003] However, in the traditional production of polyurethane synthetic leather, polyurethane resins with organic solvents are used as the base and surface layers of leather products. This type of polyurethane resin is prepared by polymerization using toluene, xylene, acetone, butanone, acetic acid, ethyl ester and dimethylformamide as the main solvents. These solvents have great toxic side effects, not only causing environmental pollution and harming the body, but also being flammable and explosive, and easily causing fire and other accidents.
[0004] In recent years, the product structure of domestic artificial leather and synthetic leather industry has been continuously optimized, and the industry upgrade speed has accelerated. Waterborne polyurethane uses water as a medium, and has the advantages of being non-toxic, odorless, pollution-free, and non-flammable. It is a good alternative material for traditional solvent-based polyurethane and has been widely used in many fields such as textile fabric coating, synthetic leather, natural leather finishing, adhesives, etc. The emergence of waterborne polyurethane synthetic leather has broadened the application field of synthetic leather.
[0005] However, there are still great limitations in simply using water-based polyurethane resin for synthetic leather processing. In addition, the gap between polyurethane synthetic leather and natural leather in terms of moisture absorption and breathability is still quite obvious, which is a problem that needs to be solved urgently.
[0006] The Chinese patent document with patent number CN201810850749.3 discloses a "method for preparing hygroscopic, antibacterial and water vapor permeable graphene-modified polyurethane synthetic leather", which can improve the hygroscopicity and air permeability of synthetic leather by adding graphene with a porous structure. However, its preparation process is relatively complicated and graphene is expensive, so the cost is high. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a waterproof and breathable synthetic leather and a preparation method thereof; the waterproof and breathable synthetic leather has very excellent air permeability and moisture removal performance, which can not only prevent the leather product from mildewing due to the inability of water vapor inside to escape, but also can further play an antibacterial role and increase the service life of the leather product.
[0008] In order to achieve the above object, the solution adopted by the present invention is:
[0009] A waterproof and breathable synthetic leather. The raw materials of the surface slurry of the waterproof and breathable synthetic leather include, by weight: 100 parts of waterborne polyurethane resin, 0.5-0.8 parts of crosslinking agent, 0.5-0.8 parts of air permeability aid, 1-2 parts of antibacterial activated carbon, 0.4-0.6 parts of wetting and leveling agent, and 0.1-0.3 parts of thickener.
[0010] Furthermore, in a preferred embodiment of the present invention, the preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.5-1.8 mol / L for 4-5 hours, heating and boiling until the solution is evaporated, cooling and drying.
[0011] Furthermore, in a preferred embodiment of the present invention, the raw materials of the biomass activated carbon powder include 1-2 parts of coconut shell, 1-2 parts of straw and 1-2 parts of bamboo by weight.
[0012] Furthermore, in a preferred embodiment of the present invention, the preparation of biomass activated carbon powder includes: (1) washing, drying, and crushing coconut shells, straws, and bamboos, respectively, and mixing them to obtain a premix; (2) activating the premix; (3) adding a cross-linking agent and stirring to obtain a cross-linked product; heating the cross-linked product to 650-730°C for reaction for 1-2h, acid washing, and then washing with water to neutral and drying.
[0013] Furthermore, in a preferred embodiment of the present invention, the cross-linking agent is a 22-28% glutaraldehyde solution, and the reaction is stirred for 1-2 hours.
[0014] Furthermore, in a preferred embodiment of the present invention, the weight ratio of the crosslinking agent to the premix is 0.5-0.8:1.
[0015] Furthermore, in a preferred embodiment of the present invention, the activation in step (2) comprises: adding 0.5-0.8 times its own weight of nitric acid with a concentration of 5-7 mol / L to the premix and activating at a temperature of 52-58° C. for 0.5 h.
[0016] Furthermore, in a preferred embodiment of the present invention, the pickling in step (3) comprises adding a hydrochloric acid solution with a mass fraction of 3-4%, boiling for 2-3 hours, and filtering.
[0017] Furthermore, in a preferred embodiment of the present invention, the crosslinking agent includes an aziridine crosslinking agent; and the breathable auxiliary agent includes a modified ether siloxane nonionic surfactant.
[0018] A method for preparing the above-mentioned waterproof and breathable synthetic leather includes: applying the surface slurry to release paper, putting it into an oven for heating and drying to form a polyurethane film, then applying an adhesive on the polyurethane film and laminating it with a base fabric, and peeling off the release paper after drying and curing to obtain the waterproof and breathable synthetic leather.
[0019] The waterproof and breathable synthetic leather and the preparation method thereof provided by the present invention have the following beneficial effects:
[0020] (1) The waterproof and breathable synthetic leather provided by the present invention uses water-based polyurethane, a breathable auxiliary agent and a linking agent to synergistically form micropores with uniform breathability, thereby achieving functions such as breathability, water resistance, chemical resistance, and high temperature resistance. At the same time, the antibacterial activated carbon itself has a large specific surface area and is loose and porous, with a developed pore structure, which can further disperse other raw materials of the surface slurry, and work together to significantly improve the breathability and water permeability.
[0021] (2) The waterproof and breathable synthetic leather provided by the present invention has an antibacterial biological activated carbon which is a biomass activated carbon powder that has been treated with silver. The developed pore structure of the biomass activated carbon itself can make the silver ion dispersion surface larger and more uniform, thereby having more excellent antibacterial properties, and can be used to prevent the growth of bacteria inside and outside the synthetic leather, thereby increasing the service life of the synthetic leather;
[0022] (3) The raw material of the antibacterial bio-activated carbon of the waterproof and breathable synthetic leather provided by the present invention comes from waste biomass, and the waste biomass itself has very excellent antibacterial properties, which can further prevent the synthetic leather from mildewing;
[0023] (4) Antibacterial activated carbon comes from waste biomass, which is natural, green and environmentally friendly, and waste can be recycled, which can greatly save production costs. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0025] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0026] Example 1
[0027] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0028] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0029] The preparation of biomass activated carbon powder includes:
[0030] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0031] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0032] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0033] The present embodiment provides a method for preparing waterproof and breathable synthetic leather, comprising: applying a surface slurry to release paper, placing the surface slurry in an oven for heating and drying to form a polyurethane film, then applying an adhesive to the polyurethane film and laminating the film with a base fabric, and peeling off the release paper after drying and curing to obtain the waterproof and breathable synthetic leather.
[0034] Example 2
[0035] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.5 parts of aziridine crosslinking agent, 0.8 parts of polyether modified trisiloxane, 1 part of antibacterial activated carbon, 0.6 parts of carboxymethyl cellulose, and 0.1 parts of polyurethane.
[0036] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0037] The preparation of biomass activated carbon powder includes:
[0038] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0039] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0040] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0041] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0042] Example 3
[0043] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.8 parts of aziridine crosslinking agent, 0.5 parts of polyether modified trisiloxane, 2 parts of antibacterial activated carbon, 0.4 parts of carboxymethyl cellulose, and 0.3 parts of polyurethane S.
[0044] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0045] The preparation of biomass activated carbon powder includes:
[0046] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0047] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0048] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0049] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0050] Example 4
[0051] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0052] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a 1.5 mol / L silver nitrate aqueous solution for 5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0053] The preparation of biomass activated carbon powder includes:
[0054] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0055] (2) Activation of the premix: Add 0.7 times its own weight of 6 mol / L nitric acid to the premix and activate it at 55°C for 0.5h;
[0056] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0057] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0058] Example 5
[0059] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0060] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.8 mol / L for 4 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0061] The preparation of biomass activated carbon powder includes:
[0062] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0063] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0064] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0065] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0066] Example 6
[0067] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0068] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0069] The preparation of biomass activated carbon powder includes:
[0070] (1) According to weight, 1 part of coconut shell, 2 parts of straw and 1 part of bamboo are washed, dried, crushed, and mixed to obtain a premix;
[0071] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0072] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0073] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0074] Example 7
[0075] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0076] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0077] The preparation of biomass activated carbon powder includes:
[0078] (1) According to weight, 2 parts of coconut shells, 1 part of straw and 2 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0079] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0080] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0081] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0082] Example 8
[0083] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0084] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0085] The preparation of biomass activated carbon powder includes:
[0086] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0087] (2) Activating the premix: adding 0.5 times its own weight of 7 mol / L nitric acid to the premix and activating it at 52°C for 0.5 h;
[0088] (3) Add 22% glutaraldehyde solution, stir and react for 2 hours to obtain a cross-linked product, the weight ratio of the cross-linking agent to the premix is 0.5:1; heat the cross-linked product to 730°C for 1 hour, add 3% hydrochloric acid solution by mass, boil for 3 hours, filter and wash with water until neutral and dry.
[0089] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0090] Example 9
[0091] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0092] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0093] The preparation of biomass activated carbon powder includes:
[0094] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0095] (2) Activating the premix: adding 0.8 times its own weight of 5 mol / L nitric acid to the premix and activating it at 58°C for 0.5 h;
[0096] (3) Add 28% glutaraldehyde solution, stir and react for 1 hour to obtain a cross-linked product, the weight ratio of the cross-linking agent to the premix is 0.8:1; heat the cross-linked product to 650°C for 2 hours, add 4% hydrochloric acid solution by mass, boil for 2 hours, filter and wash with water until neutral and dry.
[0097] This embodiment provides a method for preparing waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0098] Comparative Example 1
[0099] The comparative example provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0100] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0101] Comparative Example 2
[0102] The comparative example provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0103] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0104] The preparation of biomass activated carbon powder includes:
[0105] (1) Washing, drying and crushing wood to obtain a premix by weight;
[0106] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0107] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0108] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0109] Comparative Examples 3-5
[0110] The comparative example provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0111] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0112] The preparation of biomass activated carbon powder includes:
[0113] (1) Wash, dry and crush coconut shell, straw or bamboo by weight to obtain a premix;
[0114] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0115] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0116] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0117] Comparative Example 6
[0118] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.4 parts of aziridine crosslinking agent, 1 part of polyether modified trisiloxane, 0.5 parts of antibacterial activated carbon, 0.8 parts of carboxymethyl cellulose, and 0.4 parts of polyurethane.
[0119] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0120] The preparation of biomass activated carbon powder includes:
[0121] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0122] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0123] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0124] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0125] Comparative Example 7
[0126] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0127] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.2 mol / L for 6 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0128] The preparation of biomass activated carbon powder includes:
[0129] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0130] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0131] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0132] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0133] Comparative Example 8
[0134] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.5 parts of aziridine crosslinking agent, 0.8 parts of polyether modified trisiloxane, 1 part of antibacterial activated carbon, 0.6 parts of carboxymethyl cellulose, and 0.1 parts of polyurethane.
[0135] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0136] The preparation of biomass activated carbon powder includes:
[0137] (1) By weight, 0.8 parts of coconut shell, 2.5 parts of straw and 0.8 parts of bamboo are washed, dried, crushed, and mixed to obtain a premix;
[0138] (2) Activating the premix: adding 0.7 times its own weight of 6 mol / L nitric acid to the premix and activating it at 55°C for 0.5 h;
[0139] (3) Add 25% glutaraldehyde solution, stir and react for 1.5 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 0.7:1; heat the cross-linked product to 690°C and react for 1.5 hours, then add 3.5% hydrochloric acid solution by mass, boil for 2.5 hours, filter and wash with water until neutral and dry.
[0140] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0141] Comparative Example 9
[0142] The present embodiment provides a waterproof and breathable synthetic leather, the raw materials of the surface slurry of which include: 100 parts of waterborne polyurethane resin, 0.7 parts of aziridine crosslinking agent, 0.6 parts of polyether modified trisiloxane, 1.5 parts of antibacterial activated carbon, 0.5 parts of carboxymethyl cellulose, and 0.2 parts of polyurethane.
[0143] The preparation of antibacterial activated carbon includes: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.6 mol / L for 4.5 hours, heating and boiling until the solution is evaporated to dryness, cooling and drying.
[0144] The preparation of biomass activated carbon powder includes:
[0145] (1) By weight, 1.5 parts of coconut shell, 1.2 parts of straw and 1.3 parts of bamboo are washed, dried, crushed and mixed to obtain a premix;
[0146] (2) Activating the premix: Add 4 mol / L nitric acid at a concentration of 1 times its own weight to the premix and activate it at 60°C for 0.5 h;
[0147] (3) Add 20% glutaraldehyde solution, stir and react for 3 hours to obtain a cross-linked product, where the weight ratio of the cross-linking agent to the premix is 1:1; heat the cross-linked product to 800°C and react for 0.5 hours, then add 2% hydrochloric acid solution by mass, boil for 4 hours, filter and wash with water until neutral and dry.
[0148] This comparative example provides a method for preparing a waterproof and breathable synthetic leather. The specific method is as described in Example 1.
[0149] Experimental Example 1
[0150] Experimental method: The waterproof and breathable synthetic leathers obtained in Examples 1-9 and Comparative Examples 1-9 were tested for leather performance:
[0151] (1) Air permeability test: Refer to "QB / T 2799-2006 Leather Air Permeability Determination Method" to test the air permeability of waterproof and breathable synthetic leather;
[0152] (2) Water absorption test: refer to GB / T 4689.21-2008 Physical and mechanical tests for leather - Determination of static water absorption to test the water absorption of waterproof and breathable synthetic leather;
[0153] (3) Antibacterial property test: refer to "QB / T 4341-2012 Test method and antibacterial effect of antibacterial polyurethane synthetic leather" to test the antibacterial property;
[0154] The results are shown in Table 1:
[0155] Table 1
[0156]
[0157]
[0158] It can be seen from the data in Table 1 that the waterproof and breathable synthetic leather provided by Examples 1-9 has excellent comprehensive performance, and has excellent air permeability, waterproofness, and antibacterial and mildew-proof capabilities.
[0159] In summary, the waterproof and breathable synthetic leather and the preparation method thereof provided by the present invention have very excellent air permeability and moisture removal performance, which can not only prevent the leather product from mildewing due to the inability of water vapor inside to escape, but also can further play an antibacterial role and increase the service life of the leather product.
[0160] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A waterproof and breathable synthetic leather, characterized in that: The raw materials of the surface slurry of the waterproof and breathable synthetic leather include, by weight: 100 parts of waterborne polyurethane resin, 0.5-0.8 parts of crosslinking agent, 0.5-0.8 parts of air permeability aid, 1-2 parts of antibacterial activated carbon, 0.4-0.6 parts of wetting and leveling agent, and 0.1-0.3 parts of thickener.
2. The waterproof and breathable synthetic leather according to claim 1, characterized in that: The preparation of the antibacterial activated carbon comprises: immersing biomass activated carbon powder in a silver nitrate aqueous solution with a concentration of 1.5-1.8 mol / L for 4-5 hours, heating and boiling until the solution is evaporated to dryness, cooling, and then drying.
3. The waterproof and breathable synthetic leather according to claim 1, characterized in that: In terms of weight, the raw materials of the biomass activated carbon powder include 1-2 parts of coconut shell, 1-2 parts of straw and 1-2 parts of bamboo.
4. The waterproof and breathable synthetic leather according to claim 3, characterized in that: The preparation of the biomass activated carbon powder includes: (1) washing, drying, and crushing the coconut shell, the straw, and the bamboo, respectively, and mixing them to obtain a premix; (2) activating the premix; (3) adding a crosslinking agent, and stirring to obtain a crosslinked product; heating the crosslinked product to 650-730° C. to react for 1-2 hours, and then acid-washing and water-washing to neutral drying to obtain the obtained product.
5. The waterproof and breathable synthetic leather according to claim 4, characterized in that: The cross-linking agent is a 22-28% glutaraldehyde solution, and the reaction is stirred for 1-2 hours.
6. The waterproof and breathable synthetic leather according to claim 4, characterized in that: The weight ratio of the cross-linking agent to the premix is 0.5-0.8:
1.
7. The waterproof and breathable synthetic leather according to claim 4, characterized in that: The activation in step (2) comprises: adding 0.5-0.8 times of its own weight of nitric acid with a concentration of 5-7 mol / L to the premix and activating at a temperature of 52-58° C. for 0.5 h.
8. The waterproof and breathable synthetic leather according to claim 4, characterized in that: The pickling in step (3) comprises adding a hydrochloric acid solution with a mass fraction of 3-4%, boiling for 2-3 hours, and filtering to obtain the product.
9. The waterproof and breathable synthetic leather according to claim 1, characterized in that: The cross-linking agent includes an aziridine cross-linking agent; and the air permeability aid includes a modified ether siloxane nonionic surfactant.
10. A method for preparing the waterproof and breathable synthetic leather according to any one of claims 1 to 9, characterized in that: include: The surface slurry is scraped onto release paper, and placed in an oven for heating and drying to form a polyurethane film. Then, an adhesive is scraped onto the polyurethane film and laminated to a base fabric. After drying and curing, the release paper is peeled off to obtain the product.