Solar cell, manufacturing method thereof and photovoltaic module
Through the two-stage laser-induced sintering process, the corrosion and burn-through problem when the doped polysilicon layer on the back of TOPCon solar cells is thin is solved, the cell efficiency is improved, and the recombination loss is reduced.
Patent Information
- Application Number
- CN202410955571.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
AI Technical Summary
When the doped polysilicon layer on the back of a TOPCon solar cell is thin, the metal slurry is easily corroded and burned through, resulting in large recombination losses and affecting cell efficiency.
A two-stage laser-induced sintering process is adopted. In the first stage, low power and low bias voltage are used for laser scanning, and in the second stage, higher power and bias voltage are used to reduce the burn-through of the doped polysilicon layer by the metal slurry and reduce recombination. loss.
It effectively reduces the recombination loss on the back of the solar cell, improves the cell efficiency, ensures the best laser-induced sintering effect, and avoids overburning.
Smart Images

Figure CN118763147A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a solar cell and a manufacturing method thereof, and a photovoltaic module. Background Art
[0002] With the rapid development of photovoltaic technology, the conversion efficiency of crystalline silicon solar cells has increased year by year. At present, TOPCon cells stand out with many advantages such as high efficiency and good industrial process maturity. Many manufacturers in the industry have begun to increase the research and development progress of TOPCon cells. In related technologies, the back of the TOPCon cell adopts a stacked structure of nano silicon oxide layer / doped polysilicon layer / silicon nitride layer, and finally prints metal paste on the silicon nitride layer. The doped polysilicon layer on the back of the TOPCon cell, as the core part of the TOPCon cell, has an increasingly thinner trend. This is because reducing the thickness of the doped polysilicon layer can increase the production capacity of solar cells and reduce optical parasitic absorption. However, when the thickness of the doped polysilicon layer is thin, the glass powder in the metal paste is more likely to corrode and burn through the doped polysilicon layer and then damage the tunneling oxide layer, seriously damaging the back passivation effect of the cell, resulting in large recombination losses on the back of the solar cell, affecting the efficiency of the solar cell. Summary of the invention
[0003] Based on this, it is necessary to provide a solar cell and a method for manufacturing the same, as well as a photovoltaic module that can reduce the surface recombination loss of the solar cell and has higher efficiency.
[0004] A first aspect of an embodiment of the present application provides a method for manufacturing a solar cell, comprising:
[0005] Providing a battery body, wherein a surface of a first side and a surface of a second side of the battery body are both formed with patterned metal paste, and the first side and the second side are arranged opposite to each other;
[0006] Pre-sintering the battery body so that the metal paste on the surface of the first side and the surface of the second side of the battery body forms a first pre-cured electrode and a second pre-cured electrode respectively;
[0007] A reverse bias voltage is applied to the battery body through the first precuring electrode and the second precuring electrode, and the battery body is laser scanned to sequentially perform the first stage and the second stage laser induced sintering treatments on the battery body; the laser scanning power and the bias voltage in the first stage are lower than the laser scanning power and the bias voltage in the second stage.
[0008] In one embodiment, the laser scanning power P1 in the first stage satisfies: 30W≤P1<60W, and the reverse bias voltage V1 satisfies: 5V≤V1<10V.
[0009] In one embodiment, the laser scanning power P2 in the second stage satisfies: 60W≤P2≤100W, and the reverse bias voltage V2 satisfies: 10V≤V2≤20V.
[0010] In one embodiment, the duration of the first stage is 0.8s-1.2s, and the duration of the second stage is 0.8s-1.2s.
[0011] In one embodiment, the step of applying a reverse bias voltage to the battery body through the first pre-cured electrode and the second pre-cured electrode comprises:
[0012] A first probe of an external power source is pressed against the first pre-curing electrode, and a second probe of the external power source is pressed against the second pre-curing electrode, wherein the polarities of the first probe and the second probe are opposite.
[0013] In one embodiment, the step of providing a battery body specifically includes:
[0014] forming a first doped conductive layer on a surface of a first side of the substrate and forming a passivation contact layer on a surface of a second side of the substrate;
[0015] Forming a first passivation layer and a second passivation layer on the surfaces of the first doped conductive layer and the passivation contact layer facing away from the substrate respectively;
[0016] Patterned metal pastes are respectively formed on the surfaces of the first passivation layer and the second passivation layer facing away from the substrate.
[0017] In one embodiment, in the step of pre-sintering the battery body, the first peak temperature T1 of sintering the surface of the first side of the battery body satisfies: 700℃≤T1≤750℃, and the second peak temperature T2 of sintering the surface of the second side of the battery body satisfies: 650℃≤T2≤700℃.
[0018] In one of the embodiments, in the step of pre-sintering the battery body, the first peak temperature T1 for sintering the surface of the first side of the battery body satisfies: 600°C ≤ T1 < 700°C, and the duration of the first peak temperature is 2-30s, and the second peak temperature T2 for sintering the surface of the second side of the battery body satisfies: 550°C ≤ T2 < 650°C, and the duration of the second peak temperature is 5-10s; the cooling time range is 2-5s.
[0019] In one embodiment, at least one of the metal paste on the surface of the first side and the metal paste on the surface of the second side comprises: silver powder, aluminum powder, glass powder, additives and organic carriers, and based on the total weight of the metal paste as 100%, the weight percentage of the aluminum powder is 0% to 0.5%; the weight percentage of the glass powder is 3% to 5%;
[0020] The weight percentage of lead in glass powder is 30% to 40%.
[0021] A second aspect of an embodiment of the present application provides a solar cell, which is manufactured using the above-mentioned method for manufacturing a solar cell.
[0022] A third aspect of an embodiment of the present application provides a photovoltaic assembly, comprising at least one battery string, wherein the battery string comprises at least two of the above-mentioned solar cells.
[0023] The above-mentioned solar cell and its manufacturing method, photovoltaic module have the following beneficial effects:
[0024] Since two stages of laser induced sintering are used in the laser induced sintering process, the laser scanning power and bias voltage in the first stage are lower than those in the second stage, which can ensure the best laser induced sintering effect of the first electrode on the first side, while reducing the over-burning of the second electrode on the second side.
[0025] In the first stage of laser induced sintering, there is a lower laser scanning power and bias voltage, and among the initial contact points formed by pre-sintering on the second side, at least some of the initial contact points will be sintered under the action of the laser, and over-sintering will not occur. In the second stage of laser induced sintering, even if a higher laser scanning power and bias voltage are used, the metal paste that has been laser induced sintered in the first stage will not be sintered again, which can reduce the metal paste on the second side from burning through the doped film layer on the second side of the battery body to a certain extent, reduce the recombination loss on the second side of the solar cell, and improve the efficiency of the solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] FIG1 is a schematic diagram of the structure of a solar cell provided in an embodiment of the present application;
[0027] FIG2 is a schematic diagram of a process of manufacturing a solar cell provided in an embodiment of the present application;
[0028] FIG3 is a schematic diagram of a detailed process of a method for manufacturing a solar cell provided in an embodiment of the present application;
[0029] FIG. 4 is a schematic diagram of the structure of a solar cell body in a method for manufacturing a solar cell provided in an embodiment of the present application.
[0030] Description of Figure Numbers:
[0031] 100. Solar cells;
[0032] 101. Battery body; 102. Metal slurry;
[0033] 10. substrate; 20. first doped conductive layer; 30. first passivation layer; 31. passivation film layer; 32. anti-reflection film layer; 50. first electrode; 60. passivation contact layer; 61. tunneling oxide layer; 62. polysilicon doped conductive layer; 70. second passivation layer; 80. second electrode;
[0034] F, first side; S, second side. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0036] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0038] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0039] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0040] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0041] The solar cell and its manufacturing method, and the photovoltaic module of the embodiment of the present application are described below with reference to the accompanying drawings.
[0042] FIG. 1 is a schematic diagram of the structure of a solar cell provided in an embodiment of the present application.
[0043] 1 and 2 , a first aspect of an embodiment of the present application provides a solar cell 100, comprising: a substrate 10, a first doped conductive layer 20 and a first passivation layer 30 stacked sequentially on a first side F of the substrate 10, a passivation contact layer 60 and a second passivation layer 70 stacked sequentially on a second side S of the substrate 10, wherein the doping types of the first doped conductive layer 20 and the passivation contact layer 60 are opposite, and the first side F and the second side S are arranged relative to each other.
[0044] The solar cell 100 further includes a first electrode 50 and a second electrode 80 . The first electrode 50 is disposed on the first passivation layer 30 and is in ohmic contact with the first doped conductive layer 20 . The second electrode 80 is disposed on the second passivation layer 70 and is in ohmic contact with the passivation contact layer 60 .
[0045] The solar cell 100 in the embodiment of the present application may be a TOPCon cell, or may be configured as other types of cells as required.
[0046] When the solar cell 100 is a TOPCon cell, the solar cell 100 may include an N-type cell and a P-type cell. The substrate 10 of the N-type cell is doped with an N-type element, and the first doped conductive layer 20 is doped with a P-type element. The substrate 10 of the P-type cell is doped with a P-type element, and the first doped conductive layer 20 is doped with an N-type element. The first doped conductive layer 20 is used to form a PN junction with the substrate 10. In the embodiment of the present application, the substrate 10 is an N-type substrate as an example for explanation. At this time, the first doped conductive layer 20 may be P-type doped, for example, it may be a first doped conductive layer 20 doped with a boron element (also called a P+ emitter).
[0047] The first passivation layer 30 may include a passivation film layer 31 and an anti-reflection film layer 32 sequentially stacked on the first doped conductive layer 20 .
[0048] The passivation film layer 31 may adopt a single-layer structure or a multi-layer structure, and the material may be at least one of aluminum oxide, silicon oxide, silicon nitride or silicon oxynitride.
[0049] The anti-reflection film 32 is located on the first side F of the substrate 10, that is, on the side of the solar cell 100 that receives incident light (called the front side or the light-receiving side), and has an anti-reflection effect on the front side of the solar cell 100. The anti-reflection film 32 can adopt a multi-layer structure. In the anti-reflection film 32 of the multi-layer structure, the material of each layer can be silicon oxide, silicon nitride or silicon oxynitride.
[0050] The passivation contact layer 60 includes a tunneling oxide layer 61 and a polysilicon doped conductive layer 62 sequentially stacked on the surface of the second side S of the substrate 10 . The tunneling oxide layer 61 is used to achieve interface passivation on the surface of the second side S of the substrate 10 , achieving a chemical passivation effect.
[0051] The second passivation layer 70 is stacked on the surface of the passivation contact layer 60 away from the substrate 10. The second passivation layer 70 can also adopt a single-layer or multi-layer structure. The material of the second passivation layer 70 can be silicon oxide, silicon nitride or silicon oxynitride. The reflectivity of the second side S surface of the solar cell 100 to sunlight can be reduced, and the absorption rate of sunlight can be increased. The second passivation layer 70 plays the role of passivation and anti-reflection at the same time.
[0052] It is understandable that the above-mentioned solar cell 100 can be manufactured by adopting the following solar cell manufacturing method.
[0053] FIG. 2 is a schematic flow chart of a method for manufacturing a solar cell provided in an embodiment of the present application.
[0054] 2 , a second aspect of the embodiment of the present application further provides a method for manufacturing a solar cell, comprising:
[0055] S10, providing a battery body, wherein a surface of a first side and a surface of a second side of the battery body are both formed with patterned metal paste, and the first side and the second side are arranged opposite to each other.
[0056] S20, pre-sintering the battery body so that the metal paste on the surface of the first side and the surface of the second side of the battery body forms a first pre-cured electrode and a second pre-cured electrode respectively.
[0057] S30, applying a reverse bias voltage to the battery body through the first pre-curing electrode and the second pre-curing electrode, and performing laser scanning on the battery body to sequentially perform the first stage and the second stage laser induced sintering treatment on the battery body; the laser scanning power and the bias voltage in the first stage are lower than the laser scanning power and the bias voltage in the second stage.
[0058] The battery body 101 is pre-sintered to sinter the metal paste 102 into a first pre-cured electrode and a second pre-cured electrode. The battery body 101 is then subjected to two stages of laser induced sintering to sinter the first pre-cured electrode and the second pre-cured electrode.
[0059] The above-mentioned sintering process actually separates the two steps of corrosion and contact formation in the sintering process. In the corrosion process of the film layer on the surface of the first side F of the battery body 101, compared with the prior art that only uses one sintering to form the electrode, the sintering process includes two processes: pre-sintering and laser induced sintering, that is, some stages of the sintering process in the prior art are replaced by laser induced sintering. During the laser induced sintering process, the process time for the mutual diffusion contact between the metal slurry 102 and the substrate 10 is shorter, and the temperature near the melting point will drop rapidly. In this way, the open circuit voltage can be maintained as high as possible while reducing the contact resistance and avoiding damage to the passivation contact layer 60 during the sintering process of the metal slurry 102.
[0060] In addition, since two stages of laser induced sintering are used in the laser induced sintering process, the laser scanning power and bias voltage in the first stage are lower than the laser scanning power and bias voltage in the second stage. Therefore, the best laser induced sintering effect of the first electrode on the first side can be ensured, while reducing the over-burning of the second electrode on the second side.
[0061] In the first stage of laser induced sintering, there is a lower laser scanning power and bias voltage. Among the initial contact points formed by pre-sintering on the second side, at least part of the initial contact points will be sintered under the action of the laser, and over-sintering will not occur. In the second stage of laser induced sintering, even if a higher laser scanning power and bias voltage are used, the metal paste that has been laser induced sintered in the first stage will not be sintered again, which can reduce the metal paste on the second side from burning through the doped conductive film layer on the second side of the battery body to a certain extent, reduce the recombination loss on the second side of the solar cell, and improve the efficiency of the solar cell.
[0062] In the case where the solar cell is a TOPCon cell, the method for manufacturing a solar cell according to an embodiment of the present application is used, and a two-stage laser induced sintering process is used to simultaneously obtain optimal sintered contacts between the first electrode on the first side and the second electrode on the second side. This can, to a certain extent, alleviate the problem that when the first electrode contact point reaches the optimal size, the second electrode contact point is over-sintered to exceed the thickness of the polysilicon doping layer 62, or even damage the tunneling oxide layer 61, thereby reducing the composite loss of the passivation contact layer.
[0063] In the embodiment of the present application, the laser scanning power P1 in the first stage satisfies: 30W≤P1<60W, and the reverse bias voltage V1 satisfies: 5V≤V1<10V.
[0064] Further, the laser scanning power P1 in the first stage satisfies: 40 W ≤ P1 ≤ 50 W, preferably 42 W, 45 W, or 48 W. The reverse bias voltage V1 satisfies: 6 V ≤ V1 ≤ 8 V, preferably 6.5 V, 7 V, or 7.5 V. Such an arrangement enables the initial contact point of the second pre-cured electrode on the second side to be optimally sintered.
[0065] In the embodiment of the present application, the laser scanning power P2 in the second stage satisfies: 60W≤P2≤100W, and the reverse bias voltage V2 satisfies: 10V≤V2≤20V.
[0066] Further, the laser scanning power P2 in the second stage satisfies: 70 W≤P2≤80 W, preferably 72 W, 75 W, or 78 W. The reverse bias voltage V2 satisfies: 12 V≤V2≤18 V, preferably 13 V, 14 V, 15 V, or 16 V.
[0067] In addition, in the first stage and the second stage, the wavelength range of the laser is 532nm-1064nm.
[0068] In the embodiment of the present application, the duration of the first stage is 0.8s-1.2s, and the duration of the second stage is 0.8s-1.2s. In this way, the optimal sintering contact of the second electrode on the second side can be achieved.
[0069] In specific implementation, the duration of the first stage can be any one of 0.9s, 1s, and 1.1s. The duration of the second stage can also be any one of 0.9s, 1s, and 1.1s. It is understandable that in order to keep the mass production rhythm as much as possible, the duration of the first stage and the second stage can be set to be the same.
[0070] In the embodiment of the present application, the step of applying a reverse bias voltage to the battery body 101 through the first pre-cured electrode and the second pre-cured electrode includes:
[0071] A first probe of an external power source is pressed against the first pre-curing electrode, and a second probe of the external power source is pressed against the second pre-curing electrode, wherein the polarities of the first probe and the second probe are opposite.
[0072] In specific implementation, if the substrate 10 is an N-type substrate and the first doped conductive layer 20 is a P-type, it is necessary to set the first probe as a positive electrode and the second probe as a negative electrode to achieve the purpose of applying a reverse bias voltage to the battery body 101 .
[0073] The laser scanning of the battery body 101 includes laser scanning of the first side F surface of the battery body 101 .
[0074] In the embodiment of the present application, in step S10, the step of providing a battery body 101 specifically includes:
[0075] Forming a first doped conductive layer 20 on the surface of the first side F of the substrate 10 and forming a passivation contact layer 60 on the surface of the second side S of the substrate 10;
[0076] Forming a first passivation layer 30 and a second passivation layer 70 on the surfaces of the first doped conductive layer 20 and the passivation contact layer 60 facing away from the substrate 10 respectively;
[0077] A patterned metal paste 102 is formed on the surfaces of the first passivation layer 30 and the second passivation layer 70 facing away from the substrate 10 , respectively.
[0078] In the embodiment of the present application, in the step of pre-sintering the battery body 101, the first peak temperature T1 of sintering the surface of the first side F of the battery body 101 satisfies: 700℃≤T1≤750℃, and the second peak temperature T2 of sintering the surface of the second side S of the battery body 101 satisfies: 650℃≤T2≤700℃.
[0079] Here, the first peak temperature and the second peak temperature during pre-sintering are both about 50° C.-150° C. lower than those in the prior art, which can effectively prevent the second electrode 80 from being over-burned.
[0080] In some other embodiments, in the step of pre-sintering the battery body 101, the first peak temperature T1 for sintering the surface of the first side F of the battery body 101 satisfies: 600℃≤T1<700℃, and the duration of the first peak temperature is 2-30s, and the second peak temperature T2 for sintering the surface of the second side S of the battery body 101 satisfies: 550℃≤T2<650℃, and the duration of the second peak temperature is 5-10s; the cooling time range is 2-5s.
[0081] With such a configuration, during the pre-sintering process of the metal paste 102, the cooling speed is fast after the peak temperature, which can control the overgrowth of some initial contact points and avoid over-burning. On the other hand, since the pre-sintering is performed at a lower pre-sintering temperature and a longer peak temperature holding time is used, the distribution of the initial contact points of the first pre-cured electrode and the first doped conductive layer 20 is more uniform, which can improve the process window and stability of the laser induced sintering of the first side F.
[0082] In addition, such a configuration also enables the solar cell 100 to simultaneously obtain a higher Voc value and a higher Isc value as well as a lower contact resistivity, thereby significantly improving the conversion efficiency of the solar cell.
[0083] In the embodiment of the present application, at least one of the metal paste 102 on the surface of the first side F and the metal paste 102 on the surface of the second side S comprises: silver powder, aluminum powder, glass powder, additives and an organic carrier. Based on the total weight of the metal paste 102 being 100%, the weight percentage of the aluminum powder is 0% to 0.5%; the weight percentage of the glass powder is 3% to 5%;
[0084] The weight percentage of lead in the glass powder is 30% to 40%. The metal paste with the above ratio is also referred to as low-corrosive metal paste hereinafter.
[0085] It can be understood that, here, at least one of the metal paste 102 on the surface of the first side F and the metal paste 102 on the surface of the second side S is set to the above ratio, which means that the metal paste 102 on the surface of the first side F can adopt the above ratio, or the metal paste 102 on the surface of the second side S can adopt the above ratio, or the metal paste 102 on the surface of the first side F and the metal paste 102 on the surface of the second side S can both adopt the above ratio.
[0086] Such arrangement makes the metal paste on the surface of the first side F and / or the metal paste on the surface of the first side F have low corrosivity, and can also avoid over-sintering of the first electrode 50 and / or the second electrode 80. In specific implementation, as mentioned above, the metal paste on the surface of the first side F may include a portion corresponding to the main grid of the first electrode 50 and a portion corresponding to the sub-grid of the first electrode 50, and preferably the portion corresponding to the sub-grid of the first electrode 50 adopts the metal paste of the above-mentioned proportion. Similarly, the metal paste on the surface of the second side S may include a portion corresponding to the main grid of the second electrode 80 and a portion corresponding to the sub-grid of the second electrode 80, and preferably the portion corresponding to the sub-grid of the second electrode 80 adopts the metal paste of the above-mentioned proportion.
[0087] In addition, the above adjustment can adjust the glass phase transition temperature and silver melting ability of the glass powder, improve the corrosion stability and uniformity of the metal slurry 102 on the passivation layer thereunder, and make the size and distribution of the initial contact points of the silver-silicon interface more uniform, which is beneficial to the uniform growth of the contact points during the subsequent laser induced sintering process, so that the contact resistance between the first electrode 50 and the first doped conductive layer 20 is smaller, the ohmic contact is better, and a lower metal contact composite can be obtained. At the same time, the acid resistance of the first electrode 50 is also improved, and the reliability risk of the solar cell in the subsequent use is reduced.
[0088] Figure 3 is a detailed schematic diagram of the process of manufacturing a solar cell provided in an embodiment of the present application. Figure 4 is a schematic diagram of the structure of a solar cell body in the method of manufacturing a solar cell provided in an embodiment of the present application.
[0089] A specific example is given below to illustrate the method for manufacturing a solar cell according to an embodiment of the present application. Referring to FIG3 and FIG4 , the method includes:
[0090] S101, forming a first doped conductive material layer on the surface of the first side F of the substrate 10 by a high-temperature boron diffusion process, removing the first doped conductive material layer and BSG on the side surface and the surface of the second side S of the substrate 10 by single-sided etching, and forming a first doped conductive layer 20 on the surface of the first side F of the substrate.
[0091] S102 , forming a tunnel oxide layer 61 and a polysilicon doped conductive layer 62 on the surface of the second side S of the substrate 10 by an LPCVD process, wherein the thickness of the polysilicon doped conductive layer 62 is 50 nm-100 nm.
[0092] S103 , depositing an aluminum oxide film and a silicon nitride film in sequence on the first doped conductive layer 20 to form a first passivation layer 30 , and depositing a silicon nitride film on the polysilicon doped conductive layer 62 as a second passivation layer 70 .
[0093] S104 , forming a metal paste 102 on the first passivation layer 30 and the second passivation layer 70 , and drying the metal paste 102 to form a battery body 101 , as shown in FIG. 4 .
[0094] S105, pre-sintering the battery body 101 at a relatively low temperature in a sintering furnace, wherein the first peak temperature T1 of the surface of the first side F of the battery body 101 satisfies: 700° C. ≤ T1 ≤ 750° C., and the second peak temperature T2 of the surface of the second side S of the battery body 101 satisfies: 650° C. ≤ T2 ≤ 700° C. After pre-sintering, the metal paste on the first side F of the battery body 101 is sintered into a first pre-cured electrode, and the metal paste on the second side S of the battery body 101 is sintered into a second pre-cured electrode.
[0095] S106, applying a reverse bias voltage to the battery body 101 through the first pre-cured electrode and the second pre-cured electrode, and performing laser scanning on the battery body 101, so as to sequentially perform the first stage and the second stage of laser induced sintering treatment on the battery body, and form the first pre-cured electrode and the second pre-cured electrode into the first electrode and the second electrode respectively. The laser scanning power P1 in the first stage satisfies: 30W≤P1<60W, and the reverse bias voltage V1 satisfies: 5V≤V1<10V. The laser scanning power P2 in the second stage satisfies: 60W≤P2≤100W, and the reverse bias voltage V2 satisfies: 10V≤V2≤20V. In both stages, the wavelength range of the laser is 532nm-1064nm.
[0096] S107, subjecting the battery body 101 that has undergone the above treatment to a low-temperature thermal annealing treatment for a certain period of time, wherein the process temperature range of the annealing treatment is 100°C-300°C; the annealing process time range is 5min-15min, and the low-temperature annealing process can further improve the passivation performance.
[0097] In some embodiments, in step S104 , the metal paste 102 formed on the first passivation layer 30 may also be the aforementioned low-corrosive metal paste.
[0098] It can be understood that in the above embodiment, by dividing the laser induced treatment into two stages, while ensuring that the first electrode on the first side has the best contact performance, the electrode metal composite loss of the second electrode on the second side can also be reduced. In addition, the first pre-cured electrode on the first side adopts a lower peak temperature, and the time for laser-induced silver-silicon interdiffusion to form contact during the subsequent laser induced sintering process is also shorter, which can reduce the damage of the silver-aluminum nail to the first doped conductive layer 20, that is, the emitter, to reduce the metal contact composite. While maintaining a low silver-silicon contact resistance, Voc can be increased by more than 8mV. In addition, the thickness of the polysilicon doped conductive layer 62 on the second side can be less than 60nm, which can obtain a low electrode contact resistance during the first stage of laser induced treatment, and has a good sintering process window and stability. In addition, the electrode slurry on the first side adopts a low-corrosive metal slurry, which reduces the content of aluminum and lead components. After laser induced treatment, while maintaining a good ohmic contact, the metal contact composite on the first side is reduced, and the acid resistance of the silver electrode is improved, which reduces the reliability risk of the solar cell in subsequent use.
[0099] The manufacturing method of the solar cell of the comparative example comprises:
[0100] Step H: forming a first doped conductive material layer on the surface of the first side of the substrate by a high-temperature boron diffusion process, removing the first doped conductive material layer and BSG on the side and back of the substrate by single-sided etching, and forming a first doped conductive layer on the surface of the first side of the substrate.
[0101] Step I: forming a tunnel oxide layer and a polysilicon doped conductive layer on the surface of the second side of the substrate by an LPCVD process, depositing an aluminum oxide film and a silicon nitride film on the first doped conductive layer in sequence to form a first passivation layer, and depositing a silicon nitride film on the polysilicon doped conductive layer as a second passivation layer.
[0102] Step J: Print metal paste on the surfaces of the first passivation layer and the second passivation layer facing away from the substrate respectively, dry them, and then perform pre-sintering treatment. The peak temperature T1 for sintering the first side of the substrate satisfies: 700℃≤T1≤750℃, and the peak temperature T2 for sintering the second side of the substrate satisfies: 650℃≤T2≤700℃. The metal pastes of the first passivation layer and the second passivation layer are respectively sintered into pre-cured electrodes.
[0103] Step K: Press the first probe (positive electrode) of the external power supply against the precured electrode on the first passivation layer, and press the second probe (negative electrode) of the external power supply against the precured electrode on the second passivation layer to apply a bias voltage of 10V-20V (including the endpoint value) to the battery body. Perform laser scanning on the surface of the first passivation layer, and sinter the precured electrodes on the first passivation layer and the second passivation layer into the final state of the electrode. During the sintering process, the laser wavelength is 532nm-1064nm, and the power range of the laser scanning is 60W-100W (including the endpoint value).
[0104] Step L: performing low temperature thermal annealing.
[0105] The solar cell manufactured through S101-S107 is recorded as solar cell A1, and the solar cell manufactured through comparative example step H-step L is recorded as solar cell B1. Solar cell A1 and solar cell B1 are subjected to battery performance tests, and the test results are recorded in Table 1.
[0106] Among them, Eta is the conversion efficiency; Jsc is the short-circuit current density; Voc is the open-circuit voltage; FF is the fill factor.
[0107] Table 1
[0108]
[0109] It can be seen from the above experimental results that, compared with the solar cell B1 of the comparative example, the solar cell A1 prepared by the method of the embodiment of the present application has a cell conversion efficiency increased by 0.13%, a short-circuit current density increased by 0.09, a cell open-circuit voltage increased by 0.0016 V, and a fill factor increased by about 0.06%. It can be seen that the efficiency of the solar cell A1 prepared by the method of this embodiment is higher.
[0110] In some other embodiments, in step S105, the sintering parameters can be improved as follows. Specifically, in the step of pre-sintering the battery body 101, the first peak temperature T1 for sintering the surface of the first side F of the battery body 101 satisfies: 600°C ≤ T1 < 700°C, and the duration of the first peak temperature is 2-30s. The second peak temperature T2 for sintering the surface of the second side S of the battery body 101 satisfies: 550°C ≤ T2 < 650°C, and the duration of the second peak temperature is 5-10s; the cooling time range is 2-5s.
[0111] The third aspect of the embodiment of the present application further provides a photovoltaic module, comprising at least one battery string, wherein the battery string comprises at least two aforementioned solar cells 100. The solar cells 100 can be connected together by serial welding.
[0112] A fourth aspect of the embodiments of the present application further provides a photovoltaic system, comprising the above-mentioned photovoltaic component.
[0113] Photovoltaic systems can be used in photovoltaic power stations, such as ground power stations, rooftop power stations, water power stations, etc., and can also be used in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. Of course, it is understandable that the application scenarios of photovoltaic systems are not limited to this, that is to say, photovoltaic systems can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0114] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0115] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for manufacturing a solar cell, characterized in that: include: Providing a battery body, wherein a surface of a first side and a surface of a second side of the battery body are both formed with patterned metal paste, and the first side and the second side are arranged opposite to each other; Pre-sintering the battery body so that the metal paste on the surface of the first side and the surface of the second side of the battery body forms a first pre-cured electrode and a second pre-cured electrode respectively; A reverse bias voltage is applied to the battery body through the first pre-cured electrode and the second pre-cured electrode, and the battery body is laser scanned to sequentially perform first and second stage laser induced sintering treatments on the battery body; the laser scanning power and bias voltage in the first stage are lower than the laser scanning power and bias voltage in the second stage.
2. The method for manufacturing a solar cell according to claim 1, characterized in that: The laser scanning power P1 in the first stage satisfies: 30W≤P1<60W, and the reverse bias voltage V1 satisfies: 5V≤V1<10V.
3. The method for manufacturing a solar cell according to claim 2, characterized in that: The laser scanning power P2 in the second stage satisfies: 60W≤P2≤100W, and the reverse bias voltage V2 satisfies: 10V≤V2≤20V.
4. The method for manufacturing a solar cell according to claim 3, characterized in that: The duration of the first stage is 0.8s-1.2s, and the duration of the second stage is 0.8s-1.2s.
5. The method for manufacturing a solar cell according to claim 1, characterized in that: The step of applying a reverse bias voltage to the battery body through the first pre-cured electrode and the second pre-cured electrode comprises: A first probe of an external power source is pressed against the first pre-curing electrode, and a second probe of the external power source is pressed against the second pre-curing electrode, wherein the polarities of the first probe and the second probe are opposite.
6. The method for manufacturing a solar cell according to any one of claims 1 to 5, characterized in that: The step of providing a battery body specifically includes: forming a first doped conductive layer on a surface of a first side of a substrate and forming a passivation contact layer on a surface of a second side of the substrate; forming a first passivation layer and a second passivation layer respectively on the surfaces of the first doped conductive layer and the passivation contact layer facing away from the substrate; Patterned metal paste is respectively formed on the surfaces of the first passivation layer and the second passivation layer facing away from the substrate.
7. The method for manufacturing a solar cell according to any one of claims 1 to 5, characterized in that: In the step of pre-sintering the battery body, a first peak temperature T1 for sintering the surface of the first side of the battery body satisfies: 700°C≤T1≤750°C, and a second peak temperature T2 for sintering the surface of the second side of the battery body satisfies: 650°C≤T2≤700°C.
8. The method for manufacturing a solar cell according to any one of claims 1 to 5, characterized in that: In the step of pre-sintering the battery body, the first peak temperature T1 for sintering the surface of the first side of the battery body satisfies: 600°C ≤ T1 < 700°C, and the duration of the first peak temperature is 2-30s. The second peak temperature T2 for sintering the surface of the second side of the battery body satisfies: 550°C ≤ T2 < 650°C, and the duration of the second peak temperature is 5-10s; the cooling time range is 2-5s.
9. The method for manufacturing a solar cell according to any one of claims 1 to 5, characterized in that: At least one of the metal paste on the surface of the first side and the metal paste on the surface of the second side comprises: silver powder, aluminum powder, glass powder, additives and organic carriers, and based on the total weight of the metal paste as 100%, the weight percentage of the aluminum powder is 0% to 0.5%; the weight percentage of the glass powder is 3% to 5%; The weight percentage of lead in the glass powder is 30% to 40%.
10. A solar cell, characterized in that: The solar cell is manufactured by the manufacturing method of any one of claims 1 to 9.
11. A photovoltaic module, characterized in that: The method comprises at least one battery string, wherein the battery string comprises at least two solar cells according to claim 10.
Citation Information
Patent Citations
Preparation process of solar cell
CN113782641A
Solar cell piece laser-induced sintering method and solar cell
CN117374153A
Solar cell, preparation method thereof and photovoltaic module
CN118073467A
Cited By
Electric field enhanced light injection method and device and battery piece production method and system
CN119153589A