Coating modified positive electrode material, preparation method of coating modified positive electrode material, positive electrode plate, lithium ion battery and power utilization device

The lithium nickel manganate material is coated with lithium aluminum titanate material to form a coherent interface, which solves the problems of capacity fading and impedance increase during the cycling of lithium nickel manganate material, improves the electrochemical performance and rate performance of the material, and ensures Stability of cladding materials.

CN118763207APending Publication Date: 2024-10-11TIANJIN B&M SCI & TECH LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411171309.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Lithium nickel manganese oxide materials have problems with capacity fading and impedance increase during cycling, which limits their further application. Existing coating materials tend to be weakly bonded to the matrix, resulting in poor coating integrity, which affects material performance.

Method used

The lithium nickel manganate material is coated with lithium aluminum titanate material, and a coherent interface is formed through roasting treatment to improve the ionic conductivity and electronic conductivity, and enhance the rate performance and cycle performance of the material.

Benefits of technology

It effectively isolates the electrolyte, protects the matrix from HF erosion, reduces capacity attenuation and impedance increase, improves cycle performance and rate performance, and ensures that the coating material does not fall off easily during cycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a coating modified positive electrode material, a preparation method of the coating modified positive electrode material, a positive electrode plate, a lithium ion battery and an electric device, the coating modified positive electrode material comprises a matrix containing lithium nickel manganese oxide and a coating layer coating at least part of the surface of the matrix, and the coating layer comprises a lithium aluminum titanate material, the chemical formula of the lithium aluminum titanate material is LixAlyTizOx / 2 + 3y / 2 + 2z, x is more than 0.8 and less than 1.1, y is more than 0.9 and less than 1.1, and z is more than 0.9 and less than 1.1. Through coating modification, the cycle performance of the material can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a coated modified positive electrode material, a preparation method of the coated modified positive electrode material, a positive electrode sheet, a lithium-ion battery and an electrical device. Background Art

[0002] As the secondary battery with the best comprehensive performance at present, lithium-ion batteries are widely used in 3C products, electric vehicles, electric bicycles, energy storage and other fields due to their high specific energy, long cycle life and good safety.

[0003] Since the cathode material plays a decisive role in the performance, safety and cost of lithium-ion batteries, the selection of cathode materials is crucial. 0.5 Mn 1.5 The theoretical discharge capacity of LNMO (lithium ion oxide, lithium ion oxide) materials can reach 146.7 mA·h / g, and they have the advantages of high voltage platform, fast three-dimensional lithium ion diffusion channel, and abundant and relatively cheap price. Therefore, they have become one of the most promising high-voltage positive electrode materials.

[0004] However, lithium nickel manganese oxide materials have poor cycling performance during the cycling process, which limits their further application. Summary of the invention

[0005] Based on this, the present application provides a coated modified positive electrode material, a preparation method of the coated modified positive electrode material, a positive electrode plate, a lithium ion battery and an electrical device to improve the cycle performance of the material.

[0006] The first aspect of the present application provides a coated modified positive electrode material, comprising:

[0007] a substrate comprising lithium nickel manganese oxide; and

[0008] The coating layer is coated on at least part of the surface of the substrate, and the coating layer comprises a lithium aluminum titanate material, wherein the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0009] In some embodiments, the coated modified positive electrode material has one or more of the following features (1)-(5):

[0010] (1) The chemical formula of the lithium nickel manganese oxide is Li 1+a Ni 0.5-b Mn1.5-c M d O4, M element includes one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1;

[0011] (2) The average particle size D50 of the matrix is ​​3 μm-8 μm;

[0012] (3) The specific surface area of ​​the substrate is 0.3 m 2 / g -1.5m 2 / g;

[0013] (4) The mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):1;

[0014] (5) The average particle size D50 of the coated modified positive electrode material is 3 μm-8 μm.

[0015] The second aspect of the present application provides a method for preparing a coated modified positive electrode material, comprising the following steps:

[0016] The substrate is mixed with a lithium source, a titanium source and an aluminum source and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare the coated modified positive electrode material;

[0017] Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0018] In some embodiments, the preparation method includes at least one of the following conditions:

[0019] (1) The lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0020] (2) The titanium source includes one or more Ti-containing compounds containing Ti-O bonds;

[0021] Optionally, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate and titanyl sulfate;

[0022] (3) the aluminum source comprises one or more of an Al-containing compound containing an Al-O bond and an ionic compound containing aluminum ions;

[0023] Optionally, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide and aluminum nitrate;

[0024] (4) The temperature of the first calcination treatment is 400°C-900°C, the time is 4h-10h, and the heating rate is 1°C / min-5°C / min;

[0025] Optionally, the temperature of the first calcination treatment is 500° C.-700° C.;

[0026] (5) In the coated modified positive electrode material, the mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):1.

[0027] In some embodiments, the chemical formula of the lithium nickel manganese oxide contained in the matrix is ​​Li 1+a Ni 0.5- b Mn 1.5-c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0028] In some embodiments, the method for preparing the substrate comprises:

[0029] A nickel-manganese precursor and a lithium salt are mixed and then subjected to a second calcination treatment; or a nickel-manganese precursor, a lithium salt and an additive are mixed and then subjected to a second calcination treatment;

[0030] Optionally, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH)2;

[0031] Optionally, the additive includes one or more of an oxide and a hydroxide containing the M element;

[0032] Optionally, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1:(0.01-0.1):(0.5-0.54);

[0033] Optionally, the nickel-manganese precursor includes one or more of hydroxide, oxalate and carbonate;

[0034] Optionally, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0035] Optionally, the temperature of the second calcination treatment is 850°C-1000°C, the time is 5h-15h, the heating rate is 1°C / min-5°C / min, the calcination atmosphere is an oxygen-containing atmosphere, and the air intake rate is 100L / min-400L / min.

[0036] The third aspect of the present application provides a method for preparing a coated modified positive electrode material, comprising the following steps:

[0037] Mixing a substrate with a solution containing a lithium source, a titanium source, and an aluminum source to prepare a mixed solution;

[0038] Removing the solvent from the mixed solution, and performing a first calcination treatment on the remaining solid to form a coating layer on at least a portion of the surface of the substrate, thereby preparing the coated modified positive electrode material;

[0039] Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0040] In some embodiments, the solvent in the mixed solution is removed by filtration or volatilization.

[0041] In some embodiments, the preparation method includes at least one of the following conditions:

[0042] (1) The lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0043] (2) The titanium source includes one or more Ti-containing compounds containing Ti-O bonds;

[0044] Optionally, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate and titanyl sulfate;

[0045] (3) the aluminum source comprises one or more of an Al-containing compound containing an Al-O bond and an ionic compound containing aluminum ions;

[0046] Optionally, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide and aluminum nitrate;

[0047] (4) The temperature of the first calcination treatment is 400°C-900°C, the time is 4h-10h, and the heating rate is 1°C / min-5°C / min;

[0048] Optionally, the temperature of the first calcination treatment is 500° C.-700° C.;

[0049] (5) In the coated modified positive electrode material, the mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):1.

[0050] In some embodiments, the chemical formula of the lithium nickel manganese oxide contained in the matrix is ​​Li 1+a Ni 0.5- b Mn 1.5-c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0051] In some embodiments, the method for preparing the substrate comprises:

[0052] A nickel-manganese precursor and a lithium salt are mixed and then subjected to a second calcination treatment; or a nickel-manganese precursor, a lithium salt and an additive are mixed and then subjected to a second calcination treatment;

[0053] Optionally, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH)2;

[0054] Optionally, the additive includes one or more of an oxide and a hydroxide containing the M element;

[0055] Optionally, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1:(0.01-0.1):(0.5-0.54);

[0056] Optionally, the nickel-manganese precursor includes one or more of hydroxide, oxalate and carbonate;

[0057] Optionally, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0058] Optionally, the temperature of the second calcination treatment is 850°C-1000°C, the time is 5h-15h, the heating rate is 1°C / min-5°C / min, the calcination atmosphere is an oxygen-containing atmosphere, and the air intake rate is 100L / min-400L / min.

[0059] The fourth aspect of the present application provides a method for preparing a coated modified positive electrode material, comprising the following steps:

[0060] The substrate and the lithium aluminum titanate material are mixed and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare the coated modified positive electrode material; the lithium aluminum titanate material is obtained by calcining a mixture of a lithium source, a titanium source and an aluminum source;

[0061] Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0062] In some embodiments, the preparation method includes at least one of the following conditions:

[0063] (1) The lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0064] (2) The titanium source includes one or more Ti-containing compounds containing Ti-O bonds;

[0065] Optionally, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate and titanyl sulfate;

[0066] (3) the aluminum source comprises one or more of an Al-containing compound containing an Al-O bond and an ionic compound containing aluminum ions;

[0067] Optionally, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide and aluminum nitrate;

[0068] (4) The temperature of the first calcination treatment is 400°C-900°C, the time is 4h-10h, and the heating rate is 1°C / min-5°C / min;

[0069] Optionally, the temperature of the first calcination treatment is 500° C.-700° C.;

[0070] (5) In the coated modified positive electrode material, the mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):1.

[0071] In some embodiments, the chemical formula of the lithium nickel manganese oxide contained in the matrix is ​​Li 1+a Ni 0.5- b Mn1.5-c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0072] In some embodiments, the method for preparing the substrate comprises:

[0073] A nickel-manganese precursor and a lithium salt are mixed and then subjected to a second calcination treatment; or a nickel-manganese precursor, a lithium salt and an additive are mixed and then subjected to a second calcination treatment;

[0074] Optionally, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH)2;

[0075] Optionally, the additive includes one or more of an oxide and a hydroxide containing the M element;

[0076] Optionally, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1:(0.01-0.1):(0.5-0.54);

[0077] Optionally, the nickel-manganese precursor includes one or more of hydroxide, oxalate and carbonate;

[0078] Optionally, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide;

[0079] Optionally, the temperature of the second calcination treatment is 850°C-1000°C, the time is 5h-15h, the heating rate is 1°C / min-5°C / min, the calcination atmosphere is an oxygen-containing atmosphere, and the air intake rate is 100L / min-400L / min.

[0080] The fifth aspect of the present application provides a positive electrode plate, comprising the coated and modified positive electrode material of the first aspect of the present application, the coated and modified positive electrode material prepared by the preparation method of the second aspect of the present application, the coated and modified positive electrode material prepared by the preparation method of the third aspect of the present application, or the coated and modified positive electrode material prepared by the preparation method of the fourth aspect of the present application.

[0081] The sixth aspect of the present application provides a lithium-ion battery, comprising the positive electrode plate of the fifth aspect of the present application.

[0082] The seventh aspect of the present application provides an electrical device, comprising the lithium-ion battery of the sixth aspect of the present application.

[0083] In some embodiments, the lithium-ion battery has at least one of the following features (1)-(4):

[0084] (1) The specific discharge capacity of the lithium ion battery is 134 mAh / g-137 mAh / g;

[0085] (2) The initial coulombic efficiency of the lithium-ion battery is 93.32%-94.05%;

[0086] (3) The cycle capacity retention rate of the lithium ion battery after 100 charge and discharge cycles at 45°C is 90.8%-95.4%;

[0087] (4) The 5C / 0.33C rate discharge retention rate of the lithium ion battery is 92.3%-96.7%.

[0088] The coated modified positive electrode material provided above uses lithium aluminum titanate material to coat a substrate containing lithium nickel manganese oxide, which can effectively isolate the electrolyte, protect the substrate from HF corrosion, and improve the electrochemical cycle performance of the positive electrode material; the lithium aluminum titanate material can also improve the ionic conductivity and electronic conductivity of the positive electrode material, effectively reduce the capacity attenuation and impedance increase during the cycle process, improve the cycle performance of the material, and improve the rate performance of the positive electrode material; in addition, the lithium aluminum titanate material and lithium nickel manganese oxide can form a coherent interface, and the coating material is not easy to fall off during the cycle process, thereby further improving the cycle performance of the positive electrode material. DETAILED DESCRIPTION

[0089] For ease of understanding of the present invention, the application will be described more fully below with reference to relevant embodiments. The following provides preferred embodiments of the application. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0090] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0091] The terms "and / or", "or / and", and "and / or" used herein include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions connected by "logical and", and also undoubtedly includes technical solutions connected by "logical or".

[0092] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0093] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0094] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0095] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0096] In this application, unless otherwise specified, the size, particle size, and diameter generally refer to the average value. In this application, "particle size" and "particle size" have the same definition, both representing the average particle size of a sphere or a spheroid.

[0097] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.

[0098] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0099] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0100] In the description of the application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0101] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0102] If there is no special explanation, all the steps of the present application can be performed sequentially or randomly, preferably sequentially.

[0103] Lithium nickel manganese oxide materials have problems with capacity attenuation and increased impedance during the cycle, which limits their further application. In the related art, element doping and surface coating are often used to modify lithium nickel manganese oxide materials. Through element doping, metal ions can enter the lattice of lithium nickel manganese oxide materials, which can achieve a stable structure and reduce capacity attenuation during the cycle. Surface coating can effectively protect lithium nickel manganese oxide materials to reduce HF corrosion and improve their cycle stability under high temperature conditions. The coating materials used for surface coating of lithium nickel manganese oxide materials mainly include ZnO, Al2O3, TiO2 and Li3PO4, among which Al-based and Ti-based have the advantages of low toxicity and low price. However, the problem is that these coating materials are prone to loose bonding with the base material and poor coating integrity, and peeling occurs during the cycle, which in turn affects the material performance.

[0104] Based on the above problems, the present application adopts lithium aluminum titanate material to coat lithium nickel manganese oxide material to prepare a coated modified positive electrode material, thereby effectively improving the ionic conductivity and electronic conductivity of the positive electrode material, and the lithium aluminum titanate material and the lithium nickel manganese oxide material can form a coherent interface, which is not easy to fall off during the cycle process, thereby improving the rate performance and cycle performance of the positive electrode material.

[0105] One or more embodiments of the present application provide a coated modified positive electrode material, comprising a substrate containing lithium nickel manganese oxide and a coating layer coated on at least a portion of the surface of the substrate, wherein the coating layer comprises a lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0106] It should be noted that the "lithium nickel manganese oxide" and "lithium nickel manganese oxide" in this context are not limited to LiNi 0.5 Mn 1.5 O4, as long as it is an oxide containing lithium, nickel and manganese, for example, an oxide containing lithium, nickel and manganese doped with other metal elements (such as transition metal elements), is within the protection scope of this application.

[0107] The coated modified positive electrode material provided in the embodiment of the present application uses a lithium aluminum titanate material to coat a substrate containing lithium nickel manganese oxide, which can effectively isolate the electrolyte, protect the substrate from HF corrosion, and improve the electrochemical cycle performance of the positive electrode material; the lithium aluminum titanate material can also improve the ionic conductivity and electronic conductivity of the positive electrode material, effectively reduce the capacity attenuation and impedance increase during the cycle process, improve the cycle performance of the material, and improve the rate performance of the positive electrode material; in addition, the lithium aluminum titanate material and the lithium nickel manganese oxide can form a coherent interface, and the coated material is not easy to fall off during the cycle process, thereby further improving the cycle performance of the positive electrode material.

[0108] It can be understood that the technical solution of the present application does not exclude the situation where the substrate and / or coating layer further includes other materials, especially the situation where the substrate further includes other positive electrode active materials and / or the coating layer further includes other coating materials.

[0109] In some embodiments, the substrate mainly comprises or contains only lithium nickel manganese oxide, and the coating layer mainly comprises or contains only a chemical formula of Li x Al y Ti z O x / 2+3y / 2+2z Represents lithium aluminum titanate material.

[0110] In some embodiments, the lithium aluminum titanate material of the coating layer is directly coated on at least a portion of the surface of the lithium nickel manganese oxide of the substrate.

[0111] It is understood that the matrix and / or coating layer may further include other materials, but the content thereof should not be such that it becomes the main component, so as to avoid affecting the coating of the lithium aluminum titanate material on the lithium nickel manganese oxide.

[0112] In some embodiments, the lithium nickel manganese oxide has a chemical formula of Li 1+a Ni 0.5-b Mn 1.5-c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0113] As a possible implementation, the average particle size D50 of the matrix is ​​3 μm-8 μm; for example, it can be but not limited to 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm or a range between any two of the above particle sizes. When the average particle size D50 of the matrix is ​​within the above range, it is beneficial for the prepared material to have higher capacity, lower impedance, and excellent cycle performance.

[0114] In some optional embodiments, the specific surface area of ​​the substrate is 0.3 m 2 / g-1.5m 2 / g; for example, but not limited to 0.3 m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g or the range between any two of the above specific surface areas, etc. When the specific surface area of ​​the substrate is within the above range, it is beneficial for the prepared material to have higher capacity, lower impedance, and excellent cycle performance.

[0115] In some exemplary embodiments, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.001-0.02):1; for example, it can be but is not limited to 0.001:1, 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1, 0.015:1, 0.016:1, 0.017:1, 0.018:1, 0.019:1, 0.02:1 or a range between any two of the above mass ratios, etc. When the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is within the above range, it can effectively reduce the corrosion of hydrofluoric acid on the matrix material, and at the same time can enhance the ionic conductivity and electronic conductivity of the material, and improve the rate performance and cycle performance.

[0116] In some optional embodiments, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.002-0.012):1.

[0117] In some optional embodiments, the average particle size D50 of the coated modified positive electrode material is 3μm-8μm; for example, it can be but not limited to 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm or a range between any two of the above particle sizes.

[0118] One or more embodiments of the present application provide a method for preparing a coated modified positive electrode material, which can prepare the above-mentioned coated modified positive electrode material. The preparation method comprises the following steps:

[0119] The substrate is mixed with a lithium source, a titanium source and an aluminum source and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare a coated modified positive electrode material; wherein the substrate comprises lithium nickel manganese oxide, the coating layer comprises a lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0120] In the prepared coated modified positive electrode material, the composition, structure and properties of the lithium nickel manganese oxide in the matrix and the lithium aluminum titanate material in the coating layer are as described above and will not be repeated in the method.

[0121] It should be noted that the "first roasting treatment", "second roasting treatment" and the like mentioned in the context are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second" and the like only serve the purpose of non-exhaustive enumeration and description, and should be understood not to constitute a closed limitation on quantity.

[0122] It can be understood that the preparation method of the coated modified formulation material provided in the embodiment of the present application can conveniently and effectively regulate the molar ratio of lithium, titanium and aluminum in the coating material; the solid phase coating method is adopted, and the synthesis process is simple; the ionic conductivity and electronic conductivity of the obtained coated modified positive electrode material can be improved, and the coated material and the matrix material can form a coherent interface. The coating material is not easy to fall off during high-temperature cycling, which can effectively improve the rate performance and high-temperature cycling performance of the material.

[0123] In some embodiments, the lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate, and lithium hydroxide.

[0124] As a possible implementation, the titanium source includes one or more Ti-containing compounds containing Ti—O bonds.

[0125] In some alternative embodiments, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate, and titanyl sulfate.

[0126] In some embodiments, the aluminum source includes one or more of an Al-containing compound containing an Al—O bond and an ionic compound containing aluminum ions.

[0127] In some exemplary embodiments, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide, and aluminum nitrate.

[0128] In some optional embodiments, the temperature of the first calcination treatment is 400°C-900°C; for example, it may be but not limited to 400°C, 430°C, 450°C, 480°C, 500°C, 530°C, 550°C, 580°C, 600°C, 630°C, 650°C, 670°C, 700°C, 730°C, 750°C, 780°C, 800°C, 830°C, 850°C, 880°C, 900°C or a range between any two of the above temperatures. When the temperature of the first calcination treatment is within the above range, a coating layer can be effectively formed on the base material, thereby improving the rate performance and high temperature cycle performance of the material.

[0129] In some optional embodiments, the temperature of the first calcination treatment is 500°C-700°C.

[0130] In some exemplary embodiments, the time of the first calcination treatment is 4 hours to 10 hours; for example, it can be but is not limited to 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours or a range between any two of the above times.

[0131] In some embodiments, the heating rate of the first calcination treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0132] It should be noted that the temperature, time and heating rate of the first calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the first calcination treatment described in this document.

[0133] In some embodiments, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.001-0.02):1; for example, it can be but not limited to 0.001:1, 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1, 0.015:1, 0.016:1, 0.017:1, 0.018:1, 0.019:1, 0.02:1 or the range between any two of the above mass ratios, etc.

[0134] In some optional embodiments, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.002-0.012):1.

[0135] In some embodiments, the lithium nickel manganese oxide contained in the matrix has a chemical formula of Li 1+a Ni 0.5-b Mn 1.5- c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0136] As a non-limiting example, the method for preparing the substrate includes: mixing a nickel-manganese precursor and a lithium salt and then performing a second calcination process.

[0137] In some optional embodiments, the method for preparing the substrate includes: mixing a nickel-manganese precursor, a lithium salt and an additive and then performing a second calcination treatment.

[0138] In some optional embodiments, the chemical formula of the nickel manganese precursor is Ni 0.25 Mn 0.75 (OH)2.

[0139] In some exemplary embodiments, the additive includes one or more of an oxide and a hydroxide containing the M element.

[0140] In some embodiments, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1: (0.01-0.1): (0.5-0.54). For example, it can be, but not limited to, 1: (0.01-0.09): (0.5-0.535), 1: (0.01-0.0.08): (0.5-0.53), 1: (0.01-0.0.07): (0.5-0.525), 1: (0.01-0.06): (0.5-0.52), 1: (0.01-0.05): (0.5-0.515) or 1: (0.01-0.04): (0.5-0.51), etc.

[0141] As a possible implementation, the nickel manganese precursor includes one or more of hydroxide, oxalate and carbonate.

[0142] In some embodiments, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide.

[0143] In some optional embodiments, the temperature of the second calcination treatment is 850°C-1000°C; for example, it can be but not limited to 850°C, 880°C, 900°C, 920°C, 950°C, 980°C, 1000°C or a range between any two of the above temperatures.

[0144] In some optional embodiments, the time of the second calcination treatment is 5h-15h; for example, it can be but not limited to 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or a range between any two of the above times.

[0145] As a possible implementation manner, the heating rate of the second roasting treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0146] In some optional embodiments, the calcination atmosphere of the second calcination process is an oxygen-containing atmosphere, such as air.

[0147] In some exemplary embodiments, the air intake rate of the second roasting treatment is 100 L / min-400 L / min; for example, it can be but not limited to 100 L / min, 130 L / min, 150 L / min, 180 L / min, 200 L / min, 230 L / min, 250 L / min, 280 L / min, 300 L / min, 330 L / min, 350 L / min, 380 L / min, 400 L / min or a range between any two of the above air intake rates, etc.

[0148] It should be noted that the temperature, time, heating rate and air intake rate of the second roasting treatment can be combined in any appropriate manner, and the four can be selected from any second roasting treatment temperature, time, heating rate and air intake rate described in this article.

[0149] One or more embodiments of the present application also provide a method for preparing a coated modified positive electrode material, which can prepare the above-mentioned coated modified positive electrode material. The preparation method specifically comprises the following steps:

[0150] The substrate is mixed with a solution containing a lithium source, a titanium source and an aluminum source to prepare a mixed solution; the solvent in the mixed solution is removed, and the remaining solid is subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare a coated modified positive electrode material; wherein the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0151] In the prepared coated modified positive electrode material, the composition, structure and properties of the lithium nickel manganese oxide in the matrix and the lithium aluminum titanate material in the coating layer are as described above and will not be repeated in the method.

[0152] It can be understood that the preparation method of the coated modified formulation material provided in the embodiment of the present application can conveniently and effectively regulate the molar ratio of lithium, titanium and aluminum metal elements in the coating material, and mixing the substrate with a solution containing a lithium source, a titanium source and an aluminum source can achieve a more uniform coating effect.

[0153] In some embodiments, the solvent in the mixed solution is removed by filtering or volatilization, thereby helping to avoid adverse effects on material properties.

[0154] In some embodiments, the lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate, and lithium hydroxide.

[0155] As a possible implementation, the titanium source includes one or more Ti-containing compounds containing Ti—O bonds.

[0156] In some alternative embodiments, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate, and titanyl sulfate.

[0157] In some embodiments, the aluminum source includes one or more of an Al-containing compound containing an Al—O bond and an ionic compound containing aluminum ions.

[0158] In some exemplary embodiments, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide, and aluminum nitrate.

[0159] In some optional embodiments, the temperature of the first calcination treatment is 400°C-900°C; for example, it may be but not limited to 400°C, 430°C, 450°C, 480°C, 500°C, 530°C, 550°C, 580°C, 600°C, 630°C, 650°C, 670°C, 700°C, 730°C, 750°C, 780°C, 800°C, 830°C, 850°C, 880°C, 900°C or a range between any two of the above temperatures. When the temperature of the first calcination treatment is within the above range, a coating layer can be effectively formed on the base material, thereby improving the rate performance and high temperature cycle performance of the material.

[0160] In some embodiments, the temperature of the first calcination treatment is 500°C-700°C.

[0161] In some exemplary embodiments, the time of the first calcination treatment is 4 hours to 10 hours; for example, it can be but is not limited to 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours or a range between any two of the above times.

[0162] In some embodiments, the heating rate of the first calcination treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0163] It should be noted that the temperature, time and heating rate of the first calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the first calcination treatment described in this document.

[0164] In some embodiments, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.001-0.02):1; for example, it can be but not limited to 0.001:1, 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1, 0.015:1, 0.016:1, 0.017:1, 0.018:1, 0.019:1, 0.02:1 or the range between any two of the above mass ratios, etc.

[0165] In some optional embodiments, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.002-0.012):1.

[0166] In some embodiments, the lithium nickel manganese oxide contained in the matrix has a chemical formula of Li 1+a Ni 0.5-b Mn 1.5- c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0167] As a non-limiting example, the method for preparing the substrate includes: mixing a nickel-manganese precursor and a lithium salt and then performing a second calcination process.

[0168] In some optional embodiments, the method for preparing the substrate includes: mixing a nickel-manganese precursor, a lithium salt and an additive and then performing a second calcination treatment.

[0169] In some optional embodiments, the chemical formula of the nickel manganese precursor is Ni0.25 Mn 0.75 (OH)2.

[0170] In some exemplary embodiments, the additive includes one or more of an oxide and a hydroxide containing the M element.

[0171] In some embodiments, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1: (0.01-0.1): (0.5-0.54). For example, it can be, but not limited to, 1: (0.01-0.09): (0.5-0.535), 1: (0.01-0.0.08): (0.5-0.53), 1: (0.01-0.0.07): (0.5-0.525), 1: (0.01-0.06): (0.5-0.52), 1: (0.01-0.05): (0.5-0.515) or 1: (0.01-0.04): (0.5-0.51), etc.

[0172] As a possible implementation, the nickel manganese precursor includes one or more of hydroxide, oxalate and carbonate.

[0173] In some embodiments, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide.

[0174] In some optional embodiments, the temperature of the second calcination treatment is 850°C-1000°C; for example, it can be but not limited to 850°C, 880°C, 900°C, 920°C, 950°C, 980°C, 1000°C or a range between any two of the above temperatures.

[0175] In some optional embodiments, the time of the second calcination treatment is 5h-15h; for example, it can be but not limited to 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or a range between any two of the above times.

[0176] As a possible implementation manner, the heating rate of the second roasting treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0177] In some optional embodiments, the calcination atmosphere of the second calcination process is an oxygen-containing atmosphere, such as air.

[0178] In some exemplary embodiments, the air intake rate of the second roasting treatment is 100 L / min-400 L / min; for example, it can be but not limited to 100 L / min, 130 L / min, 150 L / min, 180 L / min, 200 L / min, 230 L / min, 250 L / min, 280 L / min, 300 L / min, 330 L / min, 350 L / min, 380 L / min, 400 L / min or a range between any two of the above air intake rates, etc.

[0179] It should be noted that the temperature, time, heating rate and air intake rate of the second roasting treatment can be combined in any appropriate manner, and the four can be selected from any second roasting treatment temperature, time, heating rate and air intake rate described in this article.

[0180] One or more embodiments of the present application provide a method for preparing a coated modified positive electrode material, which can prepare the above-mentioned coated modified positive electrode material. The preparation method comprises the following steps:

[0181] The substrate and the lithium aluminum titanate material are mixed and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare a coated modified positive electrode material; the lithium aluminum titanate material is obtained by calcining a mixture of a lithium source, a titanium source and an aluminum source; wherein the substrate comprises lithium nickel manganese oxide, the coating layer comprises the lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1.

[0182] In the prepared coated modified positive electrode material, the composition, structure and properties of the lithium nickel manganese oxide in the matrix and the lithium aluminum titanate material in the coating layer are as described above and will not be repeated in the method.

[0183] It can be understood that the method for preparing the coated modified formulation material provided in the embodiments of the present application adopts solid phase coating and has a simple process.

[0184] In some embodiments, the solvent in the mixed solution is removed by filtering or volatilization, thereby helping to avoid adverse effects on material properties.

[0185] In some embodiments, the lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate, and lithium hydroxide.

[0186] As a possible implementation, the titanium source includes one or more Ti-containing compounds containing Ti—O bonds.

[0187] In some alternative embodiments, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate, and titanyl sulfate.

[0188] In some embodiments, the aluminum source includes one or more of an Al-containing compound containing an Al—O bond and an ionic compound containing aluminum ions.

[0189] In some exemplary embodiments, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide, and aluminum nitrate.

[0190] In some optional embodiments, the temperature of the first calcination treatment is 400°C-900°C; for example, it may be but not limited to 400°C, 430°C, 450°C, 480°C, 500°C, 530°C, 550°C, 580°C, 600°C, 630°C, 650°C, 670°C, 700°C, 730°C, 750°C, 780°C, 800°C, 830°C, 850°C, 880°C, 900°C or a range between any two of the above temperatures.

[0191] In some optional embodiments, the temperature of the first calcination treatment is 500°C-700°C.

[0192] In some exemplary embodiments, the time of the first calcination treatment is 4 hours to 10 hours; for example, it can be but is not limited to 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours or a range between any two of the above times.

[0193] In some embodiments, the heating rate of the first calcination treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0194] It should be noted that the temperature, time and heating rate of the first calcination treatment can be combined in any appropriate manner, and the three can be selected from any temperature, time and heating rate of the first calcination treatment described in this document.

[0195] In some embodiments, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.001-0.02):1; for example, it can be but not limited to 0.001:1, 0.002:1, 0.003:1, 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.01:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1, 0.015:1, 0.016:1, 0.017:1, 0.018:1, 0.019:1, 0.02:1 or the range between any two of the above mass ratios, etc.

[0196] As a possible implementation manner, in the coated modified positive electrode material, the mass ratio of lithium aluminum titanate material to lithium nickel manganese oxide is (0.002-0.012):1.

[0197] In some embodiments, the lithium nickel manganese oxide contained in the matrix has a chemical formula of Li 1+a Ni 0.5-b Mn 1.5- c M d O4, M elements include one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1.

[0198] As a non-limiting example, the method for preparing the substrate includes: mixing a nickel-manganese precursor and a lithium salt and then performing a second calcination process.

[0199] In some optional embodiments, the method for preparing the substrate includes: mixing a nickel-manganese precursor, a lithium salt and an additive and then performing a second calcination treatment.

[0200] In some optional embodiments, the chemical formula of the nickel manganese precursor is Ni 0.25 Mn 0.75 (OH)2.

[0201] In some exemplary embodiments, the additive includes one or more of an oxide and a hydroxide containing the M element.

[0202] In some embodiments, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1: (0.01-0.1): (0.5-0.54). For example, it can be, but not limited to, 1: (0.01-0.09): (0.5-0.535), 1: (0.01-0.0.08): (0.5-0.53), 1: (0.01-0.0.07): (0.5-0.525), 1: (0.01-0.06): (0.5-0.52), 1: (0.01-0.05): (0.5-0.515) or 1: (0.01-0.04): (0.5-0.51), etc.

[0203] As a possible implementation, the nickel manganese precursor includes one or more of hydroxide, oxalate and carbonate.

[0204] In some embodiments, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide.

[0205] In some optional embodiments, the temperature of the second calcination treatment is 850°C-1000°C; for example, it can be but not limited to 850°C, 880°C, 900°C, 920°C, 950°C, 980°C, 1000°C or a range between any two of the above temperatures.

[0206] In some optional embodiments, the time of the second calcination treatment is 5h-15h; for example, it can be but not limited to 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or a range between any two of the above times.

[0207] As a possible implementation manner, the heating rate of the second roasting treatment is 1°C / min-5°C / min; for example, it can be but not limited to 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min or a range between any two of the above heating rates.

[0208] In some optional embodiments, the calcination atmosphere of the second calcination process is an oxygen-containing atmosphere, such as air.

[0209] In some exemplary embodiments, the air intake rate of the second roasting treatment is 100 L / min-400 L / min; for example, it can be but not limited to 100 L / min, 130 L / min, 150 L / min, 180 L / min, 200 L / min, 230 L / min, 250 L / min, 280 L / min, 300 L / min, 330 L / min, 350 L / min, 380 L / min, 400 L / min or a range between any two of the above air intake rates, etc.

[0210] It should be noted that the temperature, time, heating rate and air intake rate of the second roasting treatment can be combined in any appropriate manner, and the four can be selected from any second roasting treatment temperature, time, heating rate and air intake rate described in this article.

[0211] One or more embodiments of the present application provide a positive electrode plate, including the coated and modified positive electrode material provided in the present application or the coated and modified positive electrode material prepared by the preparation method provided in the present application.

[0212] One or more embodiments of the present application provide a lithium-ion battery, comprising the above-mentioned positive electrode plate.

[0213] The lithium-ion battery of the present application comprises the above-mentioned coated modified positive electrode material, has a high capacity and first efficiency, and has excellent rate performance and cycle performance.

[0214] In some embodiments, the discharge specific capacity of the lithium ion battery is 134mAh / g-137mAh / g; for example, it can be but not limited to 134mAh / g, 135mAh / g, 136mAh / g, 137mAh / g or a range between any two of the above discharge specific capacities.

[0215] In some embodiments, the first coulombic efficiency of the lithium ion battery is 93.32%-94.05%; for example, it can be but not limited to 93.32%, 93.35%, 93.4%, 93.45%, 93.5%, 93.55%, 93.6%, 93.65%, 93.7%, 93.75%, 93.8%, 93.85%, 93.9%, 93.95%, 94.0%, 94.05% or the range between any two of the above first coulombic efficiencies.

[0216] As a possible implementation manner, the cycle capacity retention rate of the lithium ion battery after 100 charge and discharge cycles at 45°C is 90.8%-95.4%; for example, it can be but not limited to 90.8%, 91%, 91.2%, 91.4%, 91.6%, 91.8%, 92%, 92.2%, 92.4%, 92.6%, 92.8%, 93%, 93.2%, 93.4%, 93.6%, 93.8%, 94%, 94.2%, 94.4%, 94.6%, 94.8%, 95%, 95.2%, 95.4% or the range between any two of the above cycle capacity retention rates.

[0217] It should be noted that the test method for the cycle capacity retention rate is: at 45°C, the lithium-ion battery is charged at 1C and discharged at 1C for 100 cycles with a voltage range of 3.5V-4.9V.

[0218] In some embodiments, the 5C / 0.33C rate discharge retention rate of the lithium ion battery is 92.3%-96.7%; for example, it can be but not limited to 92.3%, 93%, 93.5%, 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97% or a range between any two of the above values.

[0219] It should be noted that the rate performance test method is: at 25°C, charge the lithium-ion battery at 0.33C, discharge at 0.33C for 1 week, and the voltage range is 3.5V-4.9V; then charge the lithium-ion battery at 0.33C, discharge at 5C for 1 week, and the voltage range is 3.5V-4.9V. One or more embodiments of the present application provide an electrical device, including the above-mentioned lithium-ion battery. The electrical device can be an electric car, an electric bicycle, an electric two-wheeled vehicle, an electric vehicle power system, an energy storage system, or a mobile storage device, etc., without specific limitation.

[0220] The electric device of the present application includes the lithium-ion battery provided by the present application, and thus has at least the same advantages as the lithium-ion battery.

[0221] The technical scheme of the present invention is described in detail below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are preferably referred to the guidance given in the present invention, and can also be carried out according to the experimental manual or conventional conditions in the art, or according to the conditions recommended by the manufacturer, or with reference to experimental methods known in the art.

[0222] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0223] 1. Preparation of positive electrode materials

[0224] Example 1

[0225] Step S1: Ni 0.25 Mn 0.75 (OH)2, TiO2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0226] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0227] Step S3, mixing the lithium nickel manganese oxide obtained in step S2 with LiOH, Al2O3 and TiO2 uniformly through the high mixer, with a rotation speed of 850r / min, a mixing time set to 20min, and mixing twice; wherein the molar ratio of LiOH, Al2O3 and TiO2 is 1:0.5:1, and the mass ratio of lithium nickel manganese oxide to TiO2 is 1:0.003.

[0228] Step S4, calcining the mixed materials in step S3 at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of the lithium aluminum titanate material contained in the coating layer is LiAlTiO4, and the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi in the coated modified positive electrode material are LiAlTiO4 and LiNi 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.007:1.

[0229] Example 2

[0230] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05O4.

[0231] Step S3: LiNO3, Al(NO3)3 and C 16 H 36 O4Ti is dissolved in anhydrous ethanol to prepare a mixed solution, in which LiNO3, Al(NO3)3 and C 16 H 36 The molar ratio of O4Ti is 1.05:1:1; lithium nickel manganese oxide is added to the mixed solution and stirred evenly, and the solvent is removed by filtering to obtain a filter cake.

[0232] Step S4, drying the filter cake obtained in step S3 under vacuum conditions at a drying temperature of 70°C for 8 hours, grinding the dried product, and calcining it at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and sieving the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of the lithium aluminum titanate material contained in the coating layer is Li 1.05 AlTiO 4.025 ; Lithium aluminum titanate material Li in the coated modified positive electrode material 1.05 AlTiO 4.025 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.005:1.

[0233] Example 3

[0234] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0235] Step S3: LiNO3, Al(NO3)3 and C 16 H 36 O4Ti is dissolved in anhydrous ethanol to prepare a mixed solution, in which LiNO3, Al(NO3)3 and C 16 H 36 The molar ratio of O4Ti is 1.05:1:1; lithium nickel manganese oxide is added to the above mixed solution and stirred evenly, and then heated to 80° C. while stirring, so that part of the ethanol evaporates to form a slurry.

[0236] Step S4, drying the slurry obtained in step S3 under vacuum conditions, the drying temperature is 70°C, the drying time is 8 hours, grinding the dried product, and roasting at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the roasted product to obtain a coated modified positive electrode material; wherein the heating rate during roasting is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of the lithium aluminum titanate material contained in the coating layer is Li 1.05 AlTiO 4.025 ; Lithium aluminum titanate material Li in the coated modified positive electrode material 1.05 AlTiO 4.025 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.005:1.

[0237] Example 4

[0238] The preparation method of Example 4 is similar to the preparation method of Example 3, with the main difference being that the temperature of calcining the ground material in step S4 of Example 4 is 600° C., and the rest are the same.

[0239] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0240] Step S3: LiNO3, Al(NO3)3 and C 16 H 36 O4Ti is dissolved in anhydrous ethanol to prepare a mixed solution, in which LiNO3, Al(NO3)3 and C 16 H 36 The molar ratio of O4Ti is 1.05:1:1; lithium nickel manganese oxide is added to the above mixed solution and stirred evenly, and then heated to 80° C. while stirring, so that part of the ethanol evaporates to form a slurry.

[0241] Step S4, drying the slurry obtained in step S3 under vacuum conditions, the drying temperature is 70°C, the drying time is 8 hours, grinding the dried product, and calcining it at 600°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and sieving the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of the lithium aluminum titanate material contained in the coating layer is Li 1.05 AlTiO 4.025; Lithium aluminum titanate material Li in the coated modified positive electrode material 1.05 AlTiO 4.025 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.005:1.

[0242] Example 5

[0243] The preparation method of Example 5 is similar to the preparation method of Example 3, with the main difference being that the temperature of calcining the ground material in step S4 of Example 5 is 500° C., and the rest are the same.

[0244] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0245] Step S3: LiNO3, Al(NO3)3 and C 16 H 36 O4Ti is dissolved in anhydrous ethanol to prepare a mixed solution, in which LiNO3, Al(NO3)3 and C 16 H 36 The molar ratio of O4Ti is 1.05:1:1; lithium nickel manganese oxide is added to the above mixed solution and stirred evenly, and then heated to 80° C. while stirring, so that part of the ethanol evaporates to form a slurry.

[0246] Step S4, drying the slurry obtained in step S3 under vacuum conditions, the drying temperature is 70°C, the drying time is 8 hours, grinding the dried product, and calcining it at 500°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and sieving the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of the lithium aluminum titanate material contained in the coating layer is Li 1.05 AlTiO 4.025 ; Lithium aluminum titanate material Li in the coated modified positive electrode material 1.05 AlTiO 4.025 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.005:1.

[0247] Example 6

[0248] The preparation method of Example 5 is similar to the preparation method of Example 3, with the main difference being that the temperature of calcining the ground material in step S4 of Example 5 is 400° C., and the rest are the same.

[0249] Example 7

[0250] The preparation method of Example 7 is similar to the preparation method of Example 3, with the main difference being that the temperature at which the ground material is calcined in step S4 of Example 7 is 900° C., and the rest are the same.

[0251] Example 8

[0252] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0253] Step S3, Al(NO3)3 and Ti(SO4)2 solutions are mixed in a molar ratio of Al to Ti of 1:1, and LiOH solution (as a pH regulator) is added under stirring to adjust the pH value of the solution to 11; after the reaction is completed, a mixture of Al and Ti hydroxides is obtained by centrifugal washing; then LiOH solution is added to the mixture, and the mixture is dried at 80°C and ground to obtain a precursor powder, in which the molar ratio of Li to Ti is 1:1.

[0254] Step S4, heating the precursor powder obtained in step S3 at 700° C. for 4 h in an air atmosphere to obtain lithium aluminum titanate material LiAlTiO4.

[0255] Step S5: LiAlTiO4 and LiNiMnO 0.5 Mn 1.45 Ti 0.05 O4 is mixed in a mass ratio of 0.002:1, and mixed evenly by a high-speed mixer at a speed of 850r / min, the mixing time is set to 20min, and mixed twice; the mixed material is roasted at 700℃ for 6h to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and the roasted product is crushed and sieved to obtain a coated modified positive electrode material; wherein the heating rate during roasting is 5℃ / min, the atmosphere is air, and the air intake rate is 200L / min. The lithium aluminum titanate material LiAlTiO4 and lithium nickel manganese oxide LiNi in the coated modified positive electrode material 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.002:1.

[0256] Example 9

[0257] The preparation method of Example 9 is similar to that of Example 8, except that: in step S5 of Example 9, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 is prepared at a mass ratio of 0.007:1, and the other ingredients are the same. The details are as follows:

[0258] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0259] Step S3, Al(NO3)3 and Ti(SO4)2 solutions are mixed in a molar ratio of Al to Ti of 1:1, and LiOH solution (as a pH regulator) is added under stirring to adjust the pH value of the solution to 11; after the reaction is completed, a mixture of Al and Ti hydroxides is obtained by centrifugal washing; then LiOH solution is added to the mixture, and the mixture is dried at 80°C and ground to obtain a precursor powder, in which the molar ratio of Li to Ti is 1:1.

[0260] Step S4, heating the precursor powder obtained in step S3 at 700° C. for 4 h in an air atmosphere to obtain lithium aluminum titanate material LiAlTiO4.

[0261] Step S5: LiAlTiO4 and LiNiMnO 0.5 Mn 1.45 Ti 0.05 O4 is mixed with a mass ratio of 0.007:1, and mixed evenly by a high-speed mixer at a speed of 850r / min, the mixing time is set to 20min, and mixed twice; the mixed material is roasted at 700℃ for 6h to form a coating layer on at least part of the surface of lithium nickel manganese oxide, and the roasted product is crushed and sieved to obtain a coated modified positive electrode material; wherein, the heating rate during roasting is 5℃ / min, the atmosphere is air, and the air intake rate is 200L / min. The lithium aluminum titanate material LiAlTiO4 and lithium nickel manganese oxide LiNi in the coated modified positive electrode material 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.007:1.

[0262] Example 10

[0263] The preparation method of Example 10 is similar to the preparation method of Example 8, except that: in step S5 of Example 10, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi0.5 Mn 1.45 Ti 0.05 O4 is prepared at a mass ratio of 0.012:1, and the other ingredients are the same. The details are as follows:

[0264] Step S1 and step S2: The same as step S1 and step S2 in Example 1, to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4.

[0265] Step S3, Al(NO3)3 and Ti(SO4)2 solutions are mixed in a molar ratio of Al to Ti of 1:1, and LiOH solution (as a pH regulator) is added under stirring to adjust the pH value of the solution to 11; after the reaction is completed, a mixture of Al and Ti hydroxides is obtained by centrifugal washing; then LiOH solution is added to the mixture, and the mixture is dried at 80°C and ground to obtain a precursor powder, in which the molar ratio of Li to Ti is 1:1.

[0266] Step S4, heating the precursor powder obtained in step S3 at 700° C. for 4 h in an air atmosphere to obtain lithium aluminum titanate material LiAlTiO4.

[0267] Step S5: LiAlTiO4 and LiNiMnO 0.5 Mn 1.45 Ti 0.05 O4 is mixed in a mass ratio of 0.012:1, and mixed evenly by a high-speed mixer at a speed of 850r / min, the mixing time is set to 20min, and mixed twice; the mixed material is roasted at 700℃ for 6h to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and the roasted product is crushed and sieved to obtain a coated modified positive electrode material; wherein the heating rate during roasting is 5℃ / min, the atmosphere is air, and the air intake rate is 200L / min. The lithium aluminum titanate material LiAlTiO4 and lithium nickel manganese oxide LiNi in the coated modified positive electrode material 0.5 Mn 1.45 Ti 0.05 The mass ratio of O4 is 0.012:1.

[0268] Embodiment 11

[0269] The preparation method of Example 11 is similar to the preparation method of Example 8, except that: in step S5 of Example 11, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 is prepared at a mass ratio of 0.001:1, and the others are the same.

[0270] Example 12

[0271] The preparation method of Example 12 is similar to the preparation method of Example 8, except that: in step S5 of Example 12, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 is prepared in a mass ratio of 0.02:1, and the others are the same.

[0272] Embodiment 13

[0273] The preparation method of Example 13 is similar to the preparation method of Example 8, except that: in step S5 of Example 13, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 is prepared in a mass ratio of 0.025:1, and the others are the same.

[0274] Embodiment 14

[0275] The preparation method of Example 14 is similar to the preparation method of Example 8, except that: in step S5 of Example 14, the lithium aluminum titanate material LiAlTiO4 and the lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 is prepared at a mass ratio of 0.0007:1, and the others are the same.

[0276] Embodiment 15

[0277] Step S1: Ni 0.25 Mn 0.75 (OH)2, Mg(OH)2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0278] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.45 Mn 1.5 Mg 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0279] Step S3, the lithium nickel manganese oxide prepared in step S2 is mixed evenly with LiOH, Al2O3 and TiO2 by the high-speed mixer, the speed is 850r / min, the mixing time is set to 20min, and the mixing is repeated twice; wherein the molar ratio of LiOH, Al2O3 and TiO2 is 1:0.5:1

[0280] Step S4, calcining the mixed materials in step S3 at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of lithium aluminum titanate contained in the coating layer is LiAlTiO4, and the coated modified positive electrode material LiAlTiO4 and lithium nickel manganese oxide LiNi 0.45 Mn 1.5 Mg 0.05 The mass ratio of O4 is 0.007:1.

[0281] Example 16

[0282] Step S1: Ni 0.25 Mn 0.75 (OH)2, Mg(OH)2, and LiOH were prepared in a molar ratio of 1:0.025:0.52, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0283] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide Li 1.04 Ni 0.45 Mn 1.5 Mg 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0284] Step S3, the lithium nickel manganese oxide prepared in step S2 is mixed evenly with LiOH, Al2O3 and TiO2 by the high-speed mixer, the speed is 850r / min, the mixing time is set to 20min, and the mixing is repeated twice; wherein the molar ratio of LiOH, Al2O3 and TiO2 is 1:0.5:1

[0285] Step S4, calcining the mixed materials in step S3 at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The chemical formula of lithium aluminum titanate contained in the coating layer is LiAlTiO4, and the LiAlTiO4 and lithium nickel manganese oxide Li in the coated modified positive electrode material are LiAlTiO4 and LiNiMnO2. 1.04 Ni 0.45 Mn 1.5 Mg 0.05 The mass ratio of O4 is 0.007:1.

[0286] Embodiment 17

[0287] Step S1: Ni 0.25 Mn 0.75 (OH)2, TiO2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0288] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0289] Step S3, the lithium nickel manganese oxide prepared in step S2 is mixed evenly with LiOH, Al2O3 and TiO2 by the high-speed mixer, the speed is 850r / min, the mixing time is set to 20min, and the mixing is repeated twice; wherein the molar ratio of LiOH, Al2O3 and TiO2 is 0.95:0.475:1.05

[0290] Step S4, calcining the mixed materials in step S3 at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The lithium aluminum titanate contained in the coating layer has a chemical formula of Li 0.95 Al 0.95 Ti 1.05 O4, Lithium aluminum titanate Li coated in the modified cathode material 0.95 Al 0.95 Ti 1.05 O4 and lithium nickel manganese oxide LiNi 0.5 Mn1.45 Ti 0.05 The mass ratio of O4 is 0.007:1.

[0291] Embodiment 18

[0292] Step S1: Ni 0.25 Mn 0.75 (OH)2, ZrO2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0293] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Zr 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0294] Step S3, the lithium nickel manganese oxide prepared in step S2 is mixed evenly with LiOH, Al2O3 and TiO2 by the high-speed mixer, the speed is 850r / min, the mixing time is set to 20min, and the mixing is repeated twice; wherein the molar ratio of LiOH, Al2O3 and TiO2 is 0.95:0.475:1.05

[0295] Step S4, calcining the mixed materials in step S3 at 700°C for 6 hours to form a coating layer on at least part of the surface of the lithium nickel manganese oxide, and crushing and screening the calcined product to obtain a coated modified positive electrode material; wherein the heating rate during calcination is 5°C / min, the atmosphere is air, and the air intake rate is 200L / min. The lithium aluminum titanate contained in the coating layer has a chemical formula of Li 0.95 Al 0.95 Ti 1.05 O4, Lithium aluminum titanate Li coated in the modified cathode material 0.95 Al 0.95 Ti 1.05 O4 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Zr 0.05 The mass ratio of O4 is 0.007:1.

[0296] Comparative Example 1

[0297] In Comparative Example 1, no coating layer was prepared, and TiO2 was not added during the preparation of lithium nickel manganese oxide. The details are as follows:

[0298] Step S1: Ni 0.25 Mn 0.75(OH)2 and LiOH were prepared in a molar ratio of 1:0.5 and mixed evenly by a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min and mixed three times to obtain a mixture after sufficient mixing.

[0299] Step S2, calcining the mixture at 850°C for 20 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.5 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0300] Comparative Example 2

[0301] No coating layer was prepared in Comparative Example 2. The details are as follows:

[0302] Step S1: Ni 0.25 Mn 0.75 (OH)2, TiO2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0303] Step S2, calcining the mixture at 850°C for 20 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0304] Comparative Example 3

[0305] Step S1: Ni 0.25 Mn 0.75 (OH)2, TiO2, and LiOH were prepared in a molar ratio of 1:0.025:0.5, and mixed evenly in a high-speed mixer at a rotation speed of 1000 r / min. The mixing time was set to 20 min, and mixed three times to obtain a mixture after sufficient mixing.

[0306] Step S2, calcining the mixture at 850°C for 10 hours, and crushing the calcined product to obtain lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; wherein, the heating rate is 3°C / min, the atmosphere is air, and the air intake rate is 200L / min.

[0307] Step S3: LiNi 0.5 Mn 1.45 Ti0.05 O4 was mixed evenly by a high-speed mixer at a rotation speed of 500 r / min, a mixing time of 10 min, and mixed once; then it was calcined at 700°C for 6 h, a heating rate of 5°C / min during calcination, an air atmosphere, and an air intake rate of 200 L / min.

[0308] Comparative Example 4

[0309] The preparation method of Comparative Example 4 is similar to that of Example 1, except that: Al2O3 is used to coat lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; others are the same. The preparation process of the coating layer is as follows:

[0310] Al2O3 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 was mixed at a mass ratio of 0.01:1 and mixed evenly by a high-speed mixer at a speed of 850 r / min for 20 min. The mixture was mixed twice and fully mixed to obtain a mixture. The mixture was calcined at 700 °C for 6 h at a heating rate of 5 °C / min in an air atmosphere at an air intake rate of 200 L / min. The calcined product was crushed and sieved to obtain an Al2O3-coated LNMO positive electrode material.

[0311] Comparative Example 5

[0312] The preparation method of Comparative Example 5 is similar to that of Example 1, except that: in Comparative Example 5, TiO2 is used to coat lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; others are the same. The preparation process of the coating layer is as follows:

[0313] TiO2 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 was mixed at a mass ratio of 0.01:1 and mixed evenly by a high-speed mixer at a speed of 850 r / min for 20 min. The mixture was mixed twice and fully mixed to obtain a mixture. The mixture was calcined at 700 ° C for 6 h at a heating rate of 5 ° C / min in an air atmosphere at an air intake rate of 200 L / min. The calcined product was crushed and sieved to obtain a TiO2-coated LNMO positive electrode material.

[0314] Comparative Example 6

[0315] The preparation method of Comparative Example 6 is similar to that of Example 1, except that: Li3PO4 is used to coat lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; others are the same. The preparation process of the coating layer is as follows:

[0316] Li3PO4 and lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4 was mixed at a mass ratio of 0.005:1 and mixed evenly by a high-speed mixer at a speed of 850 r / min for 20 min. The mixture was mixed twice and fully mixed to obtain a mixture. The mixture was calcined at 700 ° C for 6 h at a heating rate of 5 ° C / min in an air atmosphere at an air intake rate of 200 L / min. The calcined product was crushed and sieved to obtain a Li3PO4-coated LNMO positive electrode material.

[0317] Comparative Example 7

[0318] The preparation method of Comparative Example 7 is similar to that of Example 1, except that: LiNi 0.5 Mn 1.5 O4 coated lithium nickel manganese oxide LiNi 0.5 Mn 1.45 Ti 0.05 O4; others are the same. The preparation process of the coating layer is as follows:

[0319] LiNi 0.5 Mn 1.5 O4 and LiNi-MnO 0.5 Mn 1.45 Ti 0.05 O4 was mixed in a mass ratio of 0.01:1 and mixed evenly in a high-speed mixer at a speed of 850 r / min for 20 min. The mixture was mixed twice to obtain a mixture after sufficient mixing. The mixture was calcined at 700 °C for 6 h at a heating rate of 5 °C / min in an air atmosphere at an air intake rate of 200 L / min. The calcined product was crushed and sieved to obtain LiNi 0.5 Mn 1.5 O4-coated LNMO cathode material.

[0320] 2. Electrochemical performance test

[0321] The positive electrode materials, conductive agent acetylene black, and binder polyvinylidene fluoride prepared in the above embodiments and comparative examples were mixed in a mass ratio of 90:5:5, N-methylpyrrolidone was added, and the mixture was evenly mixed to form a slurry, which was coated on one side of an aluminum foil current collector. After vacuum drying, the pressed sheets were taken out and cut into positive electrode sheets of the required size.

[0322] The positive electrode sheet, lithium sheet, separator and electrolyte were assembled into a button lithium-ion battery. The assembled lithium-ion battery was subjected to rate performance test, capacity test and cycle performance test. The separator was Celgard 2500; the solvent used in the electrolyte was diethyl carbonate and ethylene carbonate in a volume ratio of 1:1, and contained 5wt% fluoroethylene carbonate, and the electrolyte was LiPF6 with a molar concentration of 1M.

[0323] The cycle performance test method is: at 45°C, charge the button battery at 1C and discharge at 1C for 100 cycles with a voltage range of 3.5V-4.9V.

[0324] The capacity test method is: at 25°C, charge the button battery at 0.33C and discharge at 0.33C for 1 week, with a voltage range of 3.5V-4.9V.

[0325] The rate performance test method is: at 25°C, charge the button battery at 0.33C and discharge at 0.33C for 1 week, with a voltage range of 3.5V-4.9V; then charge the button battery at 0.33C and discharge at 5C for 1 week, with a voltage range of 3.5V-4.9V.

[0326] The test results of the above embodiments and comparative examples are shown in Table 1.

[0327] Table 1

[0328]

[0329] From the comparison of the results of Examples 1-18 and Comparative Examples 1-7, it can be seen that compared with Comparative Examples 1-7, Examples 1-18 have higher discharge specific capacity, rate discharge retention rate and cycle capacity retention rate as a whole; this shows that the chemical formula Li x Al y Ti z O x / 2+3y / 2+2z When the lithium aluminum titanate material is used to coat and modify lithium nickel manganese oxide, the ionic conductivity and electronic conductivity of the positive electrode material can be improved, effectively reducing the capacity decay and impedance increase of the material during the cycle; and the lithium aluminum titanate material is not easy to fall off during the cycle, thereby further improving the cycle performance of the positive electrode material. Lithium-ion batteries using this positive electrode material have higher capacity and first efficiency, as well as better cycle performance.

[0330] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0331] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A coated modified positive electrode material, characterized in that: include: a substrate comprising lithium nickel manganese oxide; and The coating layer is coated on at least part of the surface of the substrate, and the coating layer comprises a lithium aluminum titanate material, wherein the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.

1.

2. The coated modified positive electrode material according to claim 1, characterized in that: The coated modified positive electrode material has one or more of the following characteristics (1)-(5): (1) The chemical formula of the lithium nickel manganese oxide is Li 1+a Ni 0.5-b Mn 1.5-c M d O4, M element includes one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1; (2) The average particle size D50 of the matrix is ​​3 μm-8 μm; (3) The specific surface area of ​​the substrate is 0.3 m 2 / g -1.5m 2 / g; (4) The mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):1; (5) The average particle size D50 of the coated modified positive electrode material is 3 μm-8 μm.

3. A method for preparing a coated modified positive electrode material, characterized in that: The steps include: The substrate is mixed with a lithium source, a titanium source and an aluminum source and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare the coated modified positive electrode material; Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1; or Mixing a substrate with a solution containing a lithium source, a titanium source, and an aluminum source to prepare a mixed solution; Removing the solvent from the mixed solution, and performing a first calcination treatment on the remaining solid to form a coating layer on at least a portion of the surface of the substrate, thereby preparing the coated modified positive electrode material; Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.1; Optionally, the solvent in the mixed solution is removed by filtering or volatilization.

4. A method for preparing a coated modified positive electrode material, characterized in that: The steps include: The substrate and the lithium aluminum titanate material are mixed and then subjected to a first calcination treatment to form a coating layer on at least a portion of the surface of the substrate to prepare the coated modified positive electrode material; the lithium aluminum titanate material is obtained by calcining a mixture of a lithium source, a titanium source and an aluminum source; Wherein, the substrate comprises lithium nickel manganese oxide, the coating layer comprises lithium aluminum titanate material, and the chemical formula of the lithium aluminum titanate material is Li x Al y Ti z O x / 2+3y / 2+2z , 0.8<x<1.1, 0.9<y<1.1, 0.9<z<1.

1.

5. The preparation method according to any one of claims 3 to 4, characterized in that: The preparation method comprises at least one of the following conditions: (1) The lithium source includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide; (2) The titanium source includes one or more Ti-containing compounds containing Ti-O bonds; Optionally, the titanium source includes one or more of titanium dioxide, tetrabutyl titanate and titanyl sulfate; (3) the aluminum source comprises one or more of an Al-containing compound containing an Al-O bond and an ionic compound containing aluminum ions; Optionally, the aluminum source includes one or more of aluminum triethoxide, aluminum oxide, aluminum hydroxide and aluminum nitrate; (4) The temperature of the first calcination treatment is 400°C-900°C, the time is 4h-10h, and the heating rate is 1°C / min-5°C / min; Optionally, the temperature of the first calcination treatment is 500° C.-700° C.; (5) In the coated modified positive electrode material, the mass ratio of the lithium aluminum titanate material to the lithium nickel manganese oxide is (0.001-0.02):1, and can be optionally (0.002-0.012):

1.

6. The preparation method according to any one of claims 3 to 4, characterized in that: The chemical formula of the lithium nickel manganese oxide contained in the matrix is ​​Li 1+a Ni 0.5-b Mn 1.5-c M d O4, M element includes one or more of Cu, Mg, Zn, Fe, Co, Al, Zr, Ti, Ru, Nb, Mo, W, Ta, B and P, -0.1<a<0.1, 0≤b<0.1, 0≤c<0.1, 0≤d<0.1; Optionally, the preparation method of the substrate comprises: A nickel-manganese precursor and a lithium salt are mixed and then subjected to a second calcination treatment; or a nickel-manganese precursor, a lithium salt and an additive are mixed and then subjected to a second calcination treatment; Optionally, the chemical formula of the nickel-manganese precursor is Ni 0.25 Mn 0.75 (OH)2; Optionally, the additive includes one or more of an oxide and a hydroxide containing the M element; Optionally, the molar ratio of the total metal elements contained in the nickel-manganese precursor, the total metal elements contained in the additive, and the lithium element contained in the lithium source is 1:(0.01-0.1):(0.5-0.54); Optionally, the nickel-manganese precursor includes one or more of hydroxide, oxalate and carbonate; Optionally, the lithium salt includes one or more of lithium carbonate, lithium nitrate, lithium chloride, lithium sulfate and lithium hydroxide; Optionally, the temperature of the second calcination treatment is 850°C-1000°C, the time is 5h-15h, the heating rate is 1°C / min-5°C / min, the calcination atmosphere is an oxygen-containing atmosphere, and the air intake rate is 100L / min-400L / min.

7. A positive electrode sheet, characterized in that: A coated and modified positive electrode material comprising the coated and modified positive electrode material as described in any one of claims 1 to 2 or a coated and modified positive electrode material prepared by the preparation method as described in any one of claims 3 to 6.

8. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as described in claim 7.

9. The lithium ion battery according to claim 8, characterized in that The lithium-ion battery has at least one of the following characteristics (1)-(4): (1) The specific discharge capacity of the lithium ion battery is 134 mAh / g-137 mAh / g; (2) The initial coulombic efficiency of the lithium-ion battery is 93.32%-94.05%; (3) The cycle capacity retention rate of the lithium ion battery after 100 charge and discharge cycles at 45°C is 90.8%-95.4%; (4) The 5C / 0.33C rate discharge retention rate of the lithium ion battery is 92.3%-96.7%.

10. An electrical device, characterized in that: Comprising a lithium ion battery as claimed in any one of claims 8 to 9.

Citation Information

Cited By

  • An additive for coating lithium battery positive electrode material and preparation method thereof

    CN119750531A